A method for preparing energy storage long cycle graphite negative electrode material
By using coke with high isotropy to prepare graphite anode materials, the problem of insufficient cycle stability of graphite anode materials in the existing technology is solved, and high-efficiency, low-cost long-cycle performance of lithium-ion batteries is achieved, which satisfies the requirements of energy storage batteries. need.
Patent Information
- Application Number
- CN202211134745.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-09-19
AI Technical Summary
Existing artificial graphite anode materials have insufficient cycle stability, complex production processes and high costs, which cannot meet the needs of reliable and low-cost chemical energy storage power stations. Their low energy density cannot meet the long cycle needs of lithium-ion batteries.
Isotropic coke with a fine mosaic structure or a small flake structure accounting for more than 50% of the area is used as raw material. Through crushing, low-temperature carbonization and graphitization, combined with demagnetization screening, a graphite anode material with high tap density and excellent performance is prepared. .
The prepared graphite anode material has high tap density, excellent first discharge efficiency and long cycle performance, which can meet the long cycle requirements of lithium-ion batteries, reduce production costs, and improve the cycle life of the battery.
Smart Images

Figure CN115477301B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of graphite negative electrode materials for lithium ion batteries, and in particular to a method for preparing an energy storage long-cycle graphite negative electrode material. Background Art
[0002] Graphite is an ideal negative electrode material and has been the dominant negative electrode material since the birth of lithium-ion batteries. The energy storage mechanism of graphite negative electrode is: through the insertion and extraction of lithium ions, graphite intercalation compounds are formed.
[0003] During the lithium insertion process of graphite, lithium ions will be embedded into graphite from the end face of the graphite layer, resulting in an increase in the distance between graphite layers. This expansion cannot be completely recovered. At the same time, the expansion of graphite materials is closely related to the cycle life of the battery. After multiple lithium insertion and de-insertion reactions, graphite materials will undergo irreversible expansion in a certain direction, which will lead to the formation of microcracks in the graphite material, the rupture and reorganization of the SEI film, the consumption of electrolyte, and the failure of cycle performance.
[0004] The amount of expansion accumulated in a certain direction of the graphite material is directly related to the orientation of the graphite. Graphite materials with a high degree of anisotropy are more likely to expand in the same direction during the lithium insertion process. Graphite materials with a high degree of isotropy can insert lithium in multiple directions, the force is more uniform, and the expansion is reduced, which is conducive to the performance of the cycle performance of the graphite material. At the same time, graphite with a high degree of isotropy has more lithium ion transmission channels and a short transmission path, which is conducive to improving rate performance.
[0005] At present, the cycle stability of artificial graphite anodes still needs to be further improved to meet the needs of reliable and low-cost chemical energy storage power stations. However, although there are many methods for preparing artificial graphite anode materials, most of these methods are improved through subsequent more complicated processes. Not only are the production processes long, the yields of each process are low, and the production costs are high, but the energy density of the prepared artificial graphite materials is low, which cannot meet the needs of long cycles of energy storage lithium-ion batteries. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a graphite negative electrode material with a long cycle and energy storage capacity in view of the technical defects in the prior art.
[0007] To this end, the present invention provides a method for preparing an energy storage long cycle graphite negative electrode material, comprising the following steps:
[0008] The first step is to crush, shape and grade the raw coke: isotropic coke with a fine mosaic structure or a small piece structure with an area of more than 50% is selected as the raw coke, and it is crushed, shaped and graded in turn to obtain a particle size D50 of 8 to 20 um and a tap density of 1.1 to 1.4 g / cm 3of coke powder;
[0009] The second step is low-temperature carbonization: carbonizing the coke powder obtained in the first step under a nitrogen atmosphere to obtain carbonized coke powder;
[0010] The third step is graphitization: the carbonized coke powder is graphitized at a temperature of 2500-2800°C. After cooling, it is demagnetized and screened to finally obtain the energy storage long-cycle graphite negative electrode material.
[0011] Preferably, in the first step, the pulverizing operation is specifically as follows: using a pulverizer, pulverizing the raw coke to a particle size D50 of 2 to 50 um, to obtain coke powder with a particle size D50 of 2 to 50 um.
[0012] Preferably, in the first step, the raw coke is isotropic coke with a fine mosaic structure or a small piece structure having an area ratio of ≥50%, an ash mass content of ≤1%, a volatile matter mass content of 8% to 15%, and a sulfur mass content of <0.5%.
[0013] Preferably, in the first step, the shaping operation specifically includes: spheroidizing the surface of the crushed coke powder, removing burrs on the surface of the coke powder, and obtaining shaped coke powder.
[0014] Preferably, in the first step, the classification operation is specifically: removing fine powder from the shaped coke powder by an air flow classifier to obtain coke powder with an average particle size D50 of 8 to 20 μm.
[0015] Preferably, in the second step, when the coke powder obtained in the first step is carbonized in a nitrogen atmosphere, the nitrogen is heated at a heating rate of 5 to 30°C / min until the temperature of the nitrogen reaches the carbonization temperature of 400 to 800°C.
[0016] Preferably, in the second step, the carbonization temperature is 400-800° C., the carbonization time is 8-72 hours, and the temperature is kept for 1-5 hours to obtain carbonized coke powder.
[0017] It can be seen from the technical solution provided by the present invention that, compared with the prior art, the present invention provides a method for preparing a long-cycle graphite negative electrode material for energy storage. The method is scientifically designed, and isotropic coke with a fine mosaic structure or a small piece structure having an area proportion of more than 50% is selected as a raw material. After treatments such as crushing, low-temperature carbonization, graphitization, and demagnetization screening, the obtained graphite negative electrode material has a higher tap density and first efficiency (first discharge efficiency). It is a long-cycle graphite negative electrode material for energy storage, which can meet the long-cycle requirements of energy storage lithium-ion batteries and has great practical significance.
[0018] After testing, the graphite negative electrode material prepared by the present invention has excellent performance parameters: particle size D50 is 8-20 μm, tap density is ≥1.1 g / cm 3 , graphite degree ≥85%, OI (orientation index) value 2~8, reversible discharge capacity ≥320mAh / g, first discharge efficiency ≥94%, 1C / 1C cycle 5000 times at room temperature, capacity retention rate ≥90%. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 A flow chart of a method for preparing an energy storage long-cycle graphite negative electrode material provided by the present invention;
[0020] Figure 2 This is a polarizing microscope photograph of the isotropic coke used in Example 1.
[0021] Figure 3 This is a polarizing microscope photograph of the isotropic coke used in Example 2;
[0022] Figure 4 This is a polarizing microscope photograph of the isotropic coke used in Example 3;
[0023] Figure 5 This is a polarizing microscope photograph of the pitch coke used in the coke of Comparative Example 1;
[0024] Figure 6 This is a polarizing microscope photograph of the petroleum coke used in Comparative Example 2. DETAILED DESCRIPTION
[0025] In order to enable those skilled in the art to better understand the scheme of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and implementation modes.
[0026] See also Figure 1 The present invention provides a method for preparing a graphite negative electrode material for energy storage and long cycle, comprising the following steps:
[0027] The first step is to crush, shape and grade the raw coke: isotropic coke with a fine mosaic structure or a small piece structure with an area of more than 50% is selected as the raw coke, and it is crushed, shaped and graded in turn to obtain a particle size D50 of 8 to 20 um and a tap density of 1.1 to 1.4 g / cm 3 of coke powder;
[0028] The second step is low-temperature carbonization: carbonizing the coke powder obtained in the first step under a nitrogen atmosphere to obtain carbonized coke powder;
[0029] In the second step, the carbonization temperature is 400-800°C, the carbonization time is 8-72 hours, and the temperature is kept at 1-5 hours.
[0030] It should be noted that the carbonization operation is carried out in a carbonization furnace. The carbonization time includes the time of the heating stage, the heat preservation stage and the cooling stage of the carbonization furnace. The sum of these three stages is the total carbonization time. The heat preservation time refers to the time for maintaining the target temperature after the temperature rises to the target temperature.
[0031] In the present invention, the heat preservation operation is to keep the temperature in the carbonization furnace for a period of time after the temperature is raised to the target temperature (specifically a temperature value between 400 and 800°C) in the early stage, in order to volatilize the light components in the coke crushed material at a certain temperature to ensure the smooth progress of the subsequent graphitization stage. The entire carbonization process is carried out in a nitrogen atmosphere. The heat preservation time is shorter than the carbonization time, and the carbonization time includes the time of the three temperature change stages.
[0032] The third step is graphitization: the carbonized coke powder is graphitized at a temperature of 2500-2800°C. After cooling, it is demagnetized and screened to finally obtain the energy storage long-cycle graphite negative electrode material.
[0033] In the present invention, in the first step, in specific implementation, the pulverizing operation is specifically: using a pulverizer, pulverizing the raw coke to a particle size D50 of 2 to 50 um, to obtain coke powder with a particle size D50 of 2 to 50 um;
[0034] It should be noted that the pulverizer used was an airflow vortex pulverizer;
[0035] In the first step, the raw coke is specifically isotropic coke with a fine mosaic structure or a small piece structure area of ≥50%, an ash mass content (i.e., mass percentage content) of ≤1%, a volatile matter mass content of 8% to 15%, and a sulfur mass content of <0.5%. Isotropic coke with these requirements can be directly provided by the coke plant.
[0036] It should be noted that, for the present invention, it is required that the area ratio of the fine mosaic structure (i.e., a specific structural area) of the coke under a polarizing microscope (i.e., the percentage of the area of the entire coke) is ≥50%, or the area ratio of the small piece structure (i.e., a specific structural area) of the coke under a polarizing microscope (i.e., the percentage of the area of the entire coke) is ≥50%.
[0037] It should be noted that in the polarizing microscope structure of coke, one color represents one orientation. Fine mosaic structure refers to a structure with a continuous size of less than 5μm of the same orientation, and small piece structure refers to a structure with a continuous size of less than 50μm of the same orientation. Ash content refers to the mass of the residue left after coke is completely burned at a certain temperature (about 800-900℃) for a period of time to constant weight. Volatile matter refers to the mass of coke after heating at 900℃ in an airtight state for 7 minutes, minus the water content of the escaping substance. Sulfur content refers to the total mass of various sulfur-containing components in coke.
[0038] In the present invention, the area ratio of the fine mosaic structure or the small piece structure in the isotropic coke is required to be ≥50%, which is conducive to the production of graphite with a high degree of isotropy, and thus the pole piece with a low degree of orientation can be prepared;
[0039] The reason why the ash content in isotropic coke is required to be ≤1% is that the more ash there is, the lower the yield of graphite from coke. More ash will reduce the quality of graphite, so reducing the ash content is to improve the yield and quality of graphite.
[0040] The reason why the mass content of volatiles in isotropic coke is required to account for 8% to 15% is that a certain amount of volatiles will form an amorphous carbon coating on the graphite surface during the low-temperature carbonization process, which is beneficial to improving the rate performance of graphite. Too little volatiles will reduce the content of amorphous carbon, and too much volatiles will affect the state of particles in the graphitization stage, making it easy for multiple particles to stick together to form secondary particles. Therefore, the volatile content is controlled within a certain range;
[0041] The reason why the mass content of sulfur in isotropic coke is required to be less than 0.5% is that if the sulfur content is too high, microporous defects will be formed inside the graphite particles after the sulfur escapes during the graphitization process, affecting the quality of the graphite. The internal defects of the graphite can easily become failure sites during the battery cycle, so the sulfur content in the coke needs to be reduced. In addition, if the sulfur content is too high, it will also cause environmental problems during the graphitization process.
[0042] It should be noted that during the charge and discharge process of lithium-ion batteries, lithium ions are embedded in the graphite layers, resulting in an increase in the interlayer spacing and expansion of the negative electrode material. This expansion is not completely recoverable. The graphite negative electrode material prepared from isotropic coke in the present invention can embed lithium in multiple directions during the charge and discharge process, the force is more uniform, and the expansion is relatively small, which is conducive to improving the cycle life of lithium-ion batteries.
[0043] In the first step, in specific implementation, the shaping operation is specifically: spheroidizing the surface of the crushed coke powder, removing the burrs on the surface of the coke powder, and obtaining the shaped coke powder;
[0044] It should be noted that the coke powder is spheroidized using a shaping machine commonly used in the art.
[0045] In the first step, the classification operation is specifically implemented as follows: the fine powder in the shaped coke powder is removed by an air flow classifier to obtain coke powder with an average particle size D50 of 8 to 20 μm.
[0046] It should be noted that, using an existing air flow classifier, the shaped coke powder can be classified to obtain coke powder with an average particle size D50 of 8 to 20 μm (ie, isotropic coke powder).
[0047] It should be noted that, through the existing air flow classifier, particles within a certain particle size range in the coke powder can be retained, and small particles and large particles can be removed. The tap density is closely related to the particle size distribution, so by controlling the particle size distribution, a specific tap density range (for example, a tap density of 1.1 to 1.4 g / cm 3 ) of coke powder.
[0048] It should be noted that the tap density is the mass per unit volume measured when the powder is in a relatively dense stacking form due to vibration. The tap density is related to the particle size distribution and morphology of graphite. The requirements for the tap density index can reflect the particle size and morphology stability of graphite to a certain extent.
[0049] In the second step, specifically, when the coke powder obtained in the first step is carbonized in a nitrogen atmosphere, the nitrogen is heated at a heating rate of 5 to 30°C / min until the temperature of the nitrogen reaches the carbonization temperature of 400 to 800°C.
[0050] It should be noted that the coke powder is carbonized under a nitrogen atmosphere to prevent the coke powder from undergoing oxidation reaction at high temperature; the heating rate is increased at 5 to 30°C / min because too fast a heating rate will cause the light components in the coke to escape too quickly, which may easily cause cracks. The heating rate is controlled to improve the stability of carbonization.
[0051] In the third step, in specific implementation, the cooled and graphitized coke powder can be demagnetized and screened by using an existing graphite demagnetizer.
[0052] It should be noted that demagnetization is to reduce the content of magnetic materials in graphite. The presence of magnetic materials will increase the self-discharge of the battery and may even cause a micro short circuit in the battery, reducing battery performance. Screening is to optimize the particle size distribution of graphite particles, remove small particles and large particles, make the particle size distribution more uniform (specifically, make the particle size D50 of the graphite negative electrode material 8-20μm), ensure the stability of the electrode preparation process, and improve the electrode quality.
[0053] In order to more clearly understand the technical solution of the present invention, the technical solution of the present invention is described below through specific embodiments.
[0054] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] Example 1.
[0056] The present invention provides a method for preparing a graphite negative electrode material for energy storage and long cycle, comprising the following preparation steps:
[0057] The first step is to crush, shape and grade the raw materials: crush the isotropic coke, shape it, grade it and remove the fine powder to obtain a particle size D50 of 11.9um and a tap density of 1.17g / cm 3 of powder;
[0058] Step 2: Low-temperature carbonization: The powder obtained by the above treatment is carbonized in a nitrogen atmosphere, the temperature is raised to 600°C at a rate of 20°C / min, and kept at this temperature for 2 hours;
[0059] Step 3: Graphitization: The carbonized powder is graphitized at 2700°C, cooled and demagnetized to obtain graphite negative electrode material.
[0060] In the first step of this embodiment, the coke adopts an isotropic coke with a fine mosaic structure or a small piece structure accounting for 60% of the area, an ash content accounting for 0.7% of the mass content, a volatile content accounting for 12% of the mass content, and a sulfur content accounting for 0.4% of the mass content. The polarizing microscope photograph of the isotropic coke is as follows: Figure 2 shown.
[0061] After inspection, the particle size D50 of the graphite negative electrode material obtained in the third step of this embodiment is 11.2 μm, and the tap density is 1.21 g / cm 3 , graphite degree is 92.5%, OI value is 3.2, reversible discharge capacity is 348.3mAh / g, first discharge efficiency is 95.3%, and capacity retention rate is 91.2% after 5000 cycles at 1C / 1C at room temperature.
[0062] Example 2.
[0063] The present invention provides a method for preparing a graphite negative electrode material for energy storage and long cycle, comprising the following preparation steps:
[0064] The first step is to crush, shape and classify the raw materials: crush, shape and classify the isotropic coke to remove fine powder, and obtain a particle size D50 of 13.2um and a tap density of 1.21g / cm 3 of powder;
[0065] Step 2: Low-temperature carbonization: The powder obtained by the above treatment is carbonized in a nitrogen atmosphere, the temperature is raised to 600°C at a rate of 20°C / min, and kept at this temperature for 2 hours;
[0066] Step 3: Graphitization: The carbonized powder is graphitized at 2700°C, cooled and demagnetized to obtain graphite negative electrode material.
[0067] In the first step of this embodiment, the coke adopts an isotropic coke with a fine mosaic structure or a small piece structure accounting for 53% of the area, an ash content accounting for 0.8% of the mass content, a volatile content accounting for 9% of the mass content, and a sulfur content accounting for 0.3% of the mass content. The polarizing microscope photo of the isotropic coke is as follows: Figure 3 shown.
[0068] After inspection, the particle size D50 of the graphite negative electrode material obtained in the third step of this embodiment is 12.4 μm, and the tap density is 1.30 g / cm 3 The graphite degree is 91.4%, the OI value is 2.8, the reversible discharge capacity is 345.9 mAh / g, the first discharge efficiency is 94.3%, and the capacity retention rate is 90.3% after 5000 cycles at 1C / 1C at room temperature.
[0069] Embodiment 3,
[0070] The present invention provides a method for preparing a graphite negative electrode material for energy storage and long cycle, comprising the following preparation steps:
[0071] Step 1: Raw material crushing, shaping and grading: The isotropic coke is crushed, shaped, graded and fine powder is removed to obtain a particle size D50 of 11.3um and a tap density of 1.12g / cm 3 of powder;
[0072] Step 2: Low-temperature carbonization: The powder obtained by the above treatment is carbonized in a nitrogen atmosphere, the temperature is raised to 600°C at a rate of 20°C / min, and kept at this temperature for 2 hours;
[0073] Step 3: Graphitization: The carbonized powder is graphitized at 2700°C, cooled and demagnetized to obtain graphite negative electrode material.
[0074] In the first step of this embodiment, the coke adopts an isotropic coke with a fine mosaic structure or a small piece structure accounting for 50% of the area, an ash content accounting for 0.3% of the mass content, a volatile content accounting for 15% of the mass content, and a sulfur content accounting for 0.4% of the mass content. The polarizing microscope photograph of the isotropic coke is as follows: Figure 4 shown.
[0075] After inspection, the particle size D50 of the graphite negative electrode material obtained in the third step of this embodiment is 10.8 μm, and the tap density is 1.18 g / cm 3 , graphite degree is 91.7%, OI value is 4.6, reversible discharge capacity is 347.7mAh / g, first discharge efficiency is 94.8%, and capacity retention rate is 90.6% after 5000 cycles at 1C / 1C at room temperature.
[0076] Comparative example 1.
[0077] An existing method for preparing a graphite negative electrode material comprises the following preparation steps:
[0078] The first step is to crush, shape and classify the raw materials: crush, shape and classify the isotropic coke to remove fine powder, and obtain a particle size D50 of 14.6um and a tap density of 1.28g / cm 3 of powder;
[0079] Step 2: Low-temperature carbonization: The powder obtained by the above treatment is carbonized in a nitrogen atmosphere, the temperature is raised to 600°C at a rate of 20°C / min, and kept at this temperature for 2 hours;
[0080] Step 3: Graphitization: The carbonized powder is graphitized at 2700°C, cooled and demagnetized to obtain graphite negative electrode material.
[0081] In the first step of this comparative example, the coke adopts a pitch coke with a fine mosaic structure or a small piece structure accounting for 7% of the area, an ash content accounting for 0.8% of the mass content, a volatile content accounting for 5% of the mass content, and a sulfur content accounting for 0.4% of the mass content. The polarizing microscope photo of the pitch coke is as follows: Figure 5 shown.
[0082] After inspection, the particle size D50 of the graphite negative electrode material obtained in the third step of this comparative example is 13.7 μm, and the tap density is 1.34 g / cm 3 The graphite degree is 90.6%, the OI value is 3.7, the reversible discharge capacity is 348.1 mAh / g, the first discharge efficiency is 94.1%, and the capacity retention rate is 82.3% after 5000 cycles at 1C / 1C at room temperature.
[0083] Comparative example 2.
[0084] An existing method for preparing a graphite negative electrode material comprises the following preparation steps:
[0085] The first step is to crush, shape and grade the raw materials: crush the isotropic coke, shape it, grade it and remove the fine powder to obtain a particle size of 15.4um and a tap density of 1.25g / cm 3 of powder;
[0086] Step 2: Low-temperature carbonization: The powder obtained by the above treatment is carbonized in a nitrogen atmosphere, the temperature is raised to 600°C at a rate of 20°C / min, and kept at this temperature for 2 hours;
[0087] Step 3: Graphitization: The carbonized powder is graphitized at 2700°C, cooled and demagnetized to obtain graphite negative electrode material.
[0088] In the first step of this comparative example, the coke adopts a domain-type polarized microstructure, has no fine mosaic and small-piece structure, and has an ash content of 0.7%, a volatile content of 10%, and a sulfur content of 0.4%. The polarized microscopic photograph of the petroleum coke is as follows: Figure 6 shown.
[0089] After inspection, the particle size D50 of the graphite negative electrode material obtained in the third step of this comparative example is 14.1 μm, and the tap density is 1.27 g / cm 3 The graphite degree is 91.8%, the OI value is 5.2, the reversible discharge capacity is 346.5mAh / g, the first discharge efficiency is 95.6%, and the capacity retention rate is 81.7% after 5000 cycles at 1C / 1C at room temperature.
[0090] The graphite negative electrode materials prepared in the above three embodiments and two comparative examples were used as negative electrode active material materials of negative electrode sheets, and further assembled into graphite-metal lithium button batteries using existing processes, and their capacity and first efficiency (first discharge efficiency) were tested, and graphite-lithium iron phosphate soft-pack batteries were assembled to test their cycle performance. The test results are shown in Table 1 below:
[0091] Table 1:
[0092]
[0093] It can be seen from Table 1 that the graphite negative electrode material prepared by the method of the present invention has a tap density of ≥1.1 g / cm 3 The above results show that the first efficiency is ≥94%, the discharge capacity is ≥320mAh / g, and the capacity retention rate of the further prepared battery after 5000 cycles at 1C / 1C at room temperature is ≥90%. It can be seen that the present invention not only meets the demand for energy storage long cycle batteries, but also has a simple preparation process, high practicality, and greatly reduces the production cost.
[0094] In summary, compared with the prior art, the method for preparing a long-cycle graphite negative electrode material for energy storage provided by the present invention is scientifically designed, and selects isotropic coke with a fine mosaic structure or a small piece structure with an area accounting for more than 50% as a raw material. After treatments such as crushing, low-temperature carbonization, graphitization, and demagnetization screening, the obtained graphite negative electrode material has a higher tap density and first efficiency (first discharge efficiency). It is a long-cycle graphite negative electrode material for energy storage, which can meet the long-cycle requirements of energy storage lithium-ion batteries and has great practical significance.
[0095] After testing, the graphite negative electrode material prepared by the present invention has excellent performance parameters: particle size D50 is 8-20 μm, tap density is ≥1.1 g / cm 3 , graphite degree ≥85%, OI (orientation index) value 2~8, reversible discharge capacity ≥320mAh / g, first discharge efficiency ≥94%, 1C / 1C cycle 5000 times at room temperature, capacity retention rate ≥90%.
[0096] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a long-cycle graphite negative electrode material for energy storage, characterized in that: The following steps are involved: The first step is to crush, shape and grade the raw coke: select isotropic coke with a fine mosaic structure or a small piece structure with an area of more than 50% as the raw coke, crush, shape and grade it in turn to obtain a particle size D50 of 8 to 20 μm and a tap density of 1.1 to 1.4 g / cm 3 of coke powder; The raw coke is specifically isotropic coke with a fine mosaic structure or a small piece structure having an area ratio of ≥50%, an ash content of ≤1%, a volatile content of 8% to 15%, and a sulfur content of <0.5%; The second step is low-temperature carbonization: the coke powder obtained in the first step is carbonized in a nitrogen atmosphere to obtain carbonized coke powder; the carbonization temperature is 400 to 800°C, the carbonization time is 8 to 72 hours, and the temperature is kept for 1 to 5 hours to obtain carbonized coke powder; The third step is graphitization: the carbonized coke powder is graphitized at a temperature of 2500-2800°C. After cooling, it is demagnetized and screened to finally obtain the energy storage long-cycle graphite negative electrode material.
2. The method for preparing the energy storage long cycle graphite negative electrode material according to claim 1, characterized in that: In the first step, the pulverizing operation is specifically as follows: the raw coke is pulverized into a particle size D50 of 2 to 50 μm by a pulverizer to obtain coke powder with a particle size D50 of 2 to 50 μm.
3. The method for preparing the energy storage long cycle graphite negative electrode material according to claim 1, characterized in that: In the first step, the shaping operation is specifically as follows: spheroidizing the surface of the crushed coke powder, removing burrs on the surface of the coke powder, and obtaining shaped coke powder.
4. The method for preparing the energy storage long cycle graphite negative electrode material according to claim 1, characterized in that: In the first step, the classification operation is specifically as follows: fine powder in the shaped coke powder is removed by an air flow classifier to obtain coke powder with an average particle size D50 of 8 to 20 μm.
5. The method for preparing the energy storage long cycle graphite negative electrode material according to any one of claims 1 to 4, characterized in that: In the second step, when the coke powder obtained in the first step is carbonized in a nitrogen atmosphere, the nitrogen is heated at a heating rate of 5 to 30°C / min until the temperature of the nitrogen reaches the carbonization temperature of 400 to 800°C.