A weaving method for double-sided different-style comfortable mini waffle fabric
By using a double-sided knitting large round machine and an improved process in the weaving process of waffle fabrics, the problems of low elasticity and quality of traditional waffle fabrics are solved, and the four-sided elastic effect and high-quality waffle fabric production are achieved.
Patent Information
- Application Number
- CN202211184426.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-09-27
AI Technical Summary
Traditional waffle fabrics have little elasticity and poor resilience, and grey fabrics are prone to problems such as holes, buckles and anti-spandex filaments during knitting.
Weaving with a double-sided knitting large circle machine, combined with improved knitting through specific knitting rules and processes, including finishing, oil removal dyeing, shaping and antibacterial treatment, using 40 combed cotton or blended yarn and 30D spandex filaments combined with improved knitting Weaving process and accessories design ensure the elastic effect and quality of the fabric on all sides.
Achieves a standard waffle fabric with four-sided elasticity, with a novel appearance, soft feel, superior elastic stretch recovery performance, no holes or buckles on the fabric, and the stretch recovery rate reaches more than 80%, enhancing the elasticity and fullness of the fabric. .
Smart Images

Figure CN115478352B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of waffle fabrics, and in particular relates to a weaving method of a double-sided comfortable mini waffle fabric with different styles. Background Art
[0002] Waffle fabric is a square or diamond-shaped concave and convex pattern, with the surface of the fabric being dark and bright. It is superior to fabrics woven from a single raw material in terms of texture, style, feel, etc., and is loved by consumers. In the prior art, a patent document with publication number CN212688349U discloses an undyed waffle fabric, which is woven using a variety of polyester yarns in different proportions. The pattern has distinct colors, improves the concave and convex feel, makes the product more beautiful, and does not require dyeing, which reduces the process, reduces costs, and is more environmentally friendly.
[0003] However, traditional waffle fabrics are stitched on both sides. Even if spandex is added, the elasticity is small and the recovery is poor, and the four-way stretch effect cannot be achieved. In addition, the grey cloth is prone to quality problems such as holes, falling buttons, and reverse spandex threads during the weaving process. Based on this, the present invention provides a weaving method for double-sided comfortable mini waffle fabrics with different styles to solve the problems raised in the above background technology. Summary of the invention
[0004] The purpose of the present invention is to provide a weaving method for double-sided comfortable mini waffle fabrics with different styles. Through a series of process settings of the weaving method, the problems of the existing waffle fabrics having low elasticity and poor recovery, failing to achieve a four-way stretch effect, and the grey cloth being prone to holes, falling off, and reverse spandex yarns during the weaving process are solved.
[0005] In order to solve the above technical problems, the present invention is achieved through the following technical solutions:
[0006] The present invention is a weaving method of a double-sided comfortable mini waffle fabric with different styles:
[0007] SS001, weaving, use double-sided knitting circular machine to weave the fabric, weave according to the following rules, with 14 routes as a cycle to form the upper and lower sides of the fabric, add spandex yarn to the needles in the 1st, 2nd, 3rd, 4th, 5th and 6th routes, and do not add spandex yarn in the 7th, 8th, 9th, 10th, 11th, 12th, 13th and 14th routes. When weaving, the upper layer of the fabric is double horizontal rows, and the knitting arrangement of the double horizontal rows in the 1st, 2nd, 3rd, 4th, 5th and 6th routes of the upper layer is a loop triangle, and the 7th, 8th, 9th, 10th, 11th, 12th, 13th and 14th routes of the upper layer are all loop triangles. The knitting arrangement of the double rows in the 14-way is all floating coils, and the lower layer of the fabric is four rows. In the lower layer, the knitting arrangement of the four rows in the 1, 2, 3, 4, 5, and 6-way is sequentially looped triangle, looped triangle, floating coil, and floating coil from the inside to the outside, and the knitting arrangement of the four rows in the 7, 9, 11, and 13-way is sequentially floating coil, looped triangle, floating coil, and looped triangle from the inside to the outside, and the knitting arrangement of the four rows in the 8, 10, 12, and 14-way is sequentially looped triangle, floating coil, looped triangle, and floating coil from the inside to the outside;
[0008] SS002, finishing, after step SS001, the woven grey cloth is obtained. After the weaving of the grey cloth is completed, the grey cloth is immersed in a finishing agent for finishing, and the raw cloth is obtained after finishing;
[0009] SS003, degreasing and dyeing, the raw cloth after step SS002 is degreased and dyed in sequence, and then dried at a low temperature within 80℃-90℃;
[0010] SS004, shaping, after step SS003, the shaping agent is evenly sprayed on the surface of the fabric treated in step SS003. After the shaping agent is sprayed, it is left to stand for 70-90 minutes. After standing, the fabric is passed through the shaping machine at a speed of 45 yards. The shaping temperature of the shaping machine is 220℃-245℃;
[0011] SS005, antibacterial treatment, the fabric after shaping is put into the antibacterial composite liquid and allowed to stand, and then the fabric is dehydrated and dried in sequence;
[0012] SS06, tail treatment, the fabric treated with antibacterial treatment in SS005 is cleaned and dried, and after drying, the fabric is sequentially subjected to shearing, ironing and cutting treatments to obtain double-sided comfortable mini waffle fabric with different styles.
[0013] Furthermore, the 1-14 routes all use 40-count combed cotton viscose yarn or blended yarn as raw material, and the spandex yarn uses 30D spandex.
[0014] Furthermore, the yarn feeding amount of the 1st, 2nd, 3rd, 4th, 5th and 6th routes is 425mm in yarn length per 100 needles, and the yarn feeding amount of the 7th to 14th routes is 215mm in yarn length per 100 needles.
[0015] Furthermore, the gasket of the lower needle cylinder in the double-sided circular knitting machine is a 120-filament gasket, and the height of the triangular needle pressing point of the needle cylinder needle floating thread coil in the double-sided circular knitting machine is 2 mm lower than the height of the triangular needle pressing point of the needle cylinder needle floating thread coil in the traditional needle cylinder needle floating thread coil, and the height of the triangular needle pressing point of the needle cylinder needle floating thread coil is marked as H.
[0016] Furthermore, the antibacterial composite liquid in the SS005 step is a mixture of an antibacterial finishing agent and deionized water of polyoxyethylene sorbitan fatty acid ester, the pH value of the antibacterial composite liquid is 6.6-6.8, and the weight percentage of the antibacterial finishing agent in the antibacterial composite liquid is 0.3%-0.55%.
[0017] Furthermore, the antibacterial finishing agent is one or a mixture of two or more of chitin, white mustard oil and chitosan.
[0018] Furthermore, the setting agent in the SS004 step includes the following raw materials in parts by weight: 8-10 parts of a color fixing agent, 6-11 parts of a stabilizer, 3-5 parts of a fatty alcohol polyoxyethylene ether, and 74-83 parts of deionized water. The color fixing agent is composed of carrageenan and polydimethyldiallylammonium chloride, and the stabilizer includes at least one of polyacrylate and sodium alginate.
[0019] Furthermore, the specific steps of finishing in the SS002 step are to soak the grey cloth twice at room temperature, boil it in the working solution for 1h-3h after removing water, and then wash it with 90℃-98℃ water for 3-5 times. During the washing process, synchronous stirring is performed, the stirring time is 20min-30min, the number of stirring times is 1-2 times, and after washing, steam heating is performed for a specified time, and then drying is performed after steam heating.
[0020] Furthermore, the working solution is composed of: 15g / L-25g / L sodium hydroxide and 0.8g / L-1.5g / L sodium chloride.
[0021] Furthermore, the specified time for the steam heating is 30 min-60 min.
[0022] The present invention has the following beneficial effects:
[0023] 1. The present invention upgrades and transforms the existing double-sided knitting circular machine and floating thread triangle accessories, invests very low research and development costs, and independently designs and develops the knitting weaving process, which expands the types of existing double-sided knitting circular machine woven fabrics. The double-sided different-style four-way stretch waffle fabric produced has a novel appearance and a soft hand feel, meets the four-way stretch standard, has excellent elastic stretch recovery performance, has no holes and buckles on the cloth surface, and has no anti-spandex defects. The produced fabric can be stretched by more than 1.7 times, and the recovery rate after stretching can reach more than 80%.
[0024] 2. The present invention uses an independently designed knitting process and improved loom accessories to weave fabrics, which not only solves the problems of holes, falling buttons and anti-spandex on the fabric surface, but also can add spandex yarns of any specifications to enhance the elasticity and fullness of the fabric, making the fabric feel more skin-friendly and soft.
[0025] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0027] Figure 1 A schematic diagram of the process structure of a weaving method for a double-sided, different-style, comfortable mini waffle fabric;
[0028] Figure 2 A schematic diagram of the structure of a triangular arrangement configuration diagram of a double-sided, different-style, comfortable mini waffle fabric;
[0029] Figure 3 It is a schematic diagram of the structure of the needle cylinder needle floating thread coil triangle pressure needle. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Embodiment 1
[0032] See also Figure 1-3 The present invention is a weaving method of a double-sided, different-style, comfortable mini waffle fabric:
[0033] SS001, weaving, using a double-sided knitting circular machine for knitting fabrics. The gasket of the lower needle cylinder in the double-sided knitting circular machine is a 120-thread gasket. Through the above-mentioned structural setting, the floating thread coils of the lower needle for 6 consecutive times are stacked neatly and are not hit by the upper needle. The height of the triangular needle pressing point of the floating thread coil of the cylinder needle in the double-sided knitting circular machine is 2mm lower than that of the triangular needle pressing point of the floating thread coil of the traditional cylinder needle. The height of the triangular needle pressing point of the floating thread coil of the cylinder needle is marked as H. Through this structural setting, the quality problems of holes, buckles and anti-spandex yarn on the cloth surface are solved;
[0034] When weaving, the following rules are followed: 14 loops are used as a loop to form the upper and lower sides of the fabric. Spandex yarn is added to the needles of the 1st, 2nd, 3rd, 4th, 5th, and 6th loops, and no spandex yarn is added to the needles of the 7th, 8th, 9th, 10th, 11th, 12th, 13th, and 14th loops. The spandex yarn is 30D spandex, that is, 9000 meters of spandex has a weight of 30 grams;
[0035] Routes 1-14 are all made of 40s combed cotton viscose yarn.
[0036] The yarn feeding amount of 1, 2, 3, 4, 5, and 6 routes is 425 mm yarn length per 100 needles, and the yarn feeding amount of 7-14 routes is 215 mm yarn length per 100 needles;
[0037] During knitting, the upper layer of the fabric is double-row, and the knitting arrangement of the double-rows in 1, 2, 3, 4, 5, and 6 routes in the upper layer is all loop triangles, and the knitting arrangement of the double-rows in 7, 8, 9, 10, 11, 12, 13, and 14 routes in the upper layer is all floating coils. The lower layer of the fabric is four-row, and in the lower layer, the knitting arrangement of the four-rows in 1, 2, 3, 4, 5, and 6 routes is loop triangle, loop triangle, floating coil, and floating coil from the inside to the outside, the knitting arrangement of the four-rows in 7, 9, 11, and 13 routes is floating coil, loop triangle, floating coil, and loop triangle from the inside to the outside, and the knitting arrangement of the four-rows in 8, 10, 12, and 14 routes is loop triangle, floating coil, loop triangle, and floating coil from the inside to the outside.
[0038] SS002, finishing. After step SS001, the woven grey cloth is obtained. After the weaving of the grey cloth is completed, the grey cloth is immersed in the finishing agent for finishing. After finishing, the raw cloth is obtained. The specific steps of finishing in step SS002 are to soak the grey cloth twice at room temperature, boil it in the working liquid for 1 hour after removing water, and then wash it with 90°C water for 3 times. During the washing process, synchronous stirring operation is performed, the stirring time is 20 minutes, the stirring number is 1, and steam heating is performed for a specified time after washing, the specified steam heating time is 30 minutes, and drying is performed after steam heating;
[0039] The working solution composition is as follows: 15 g / L sodium hydroxide, 0.8 g / L sodium chloride;
[0040] SS003, degreasing and dyeing, the raw cloth after step SS002 is degreased and dyed in sequence, and then dried at low temperature within 80°C;
[0041] SS004, shaping, after step SS003, the shaping agent is evenly sprayed on the surface of the fabric treated in step SS003. After the shaping agent is sprayed, it is left to stand for 70 minutes. After standing, the fabric is passed through the shaping machine at a speed of 45 yards. The shaping temperature of the shaping machine is 220℃;
[0042] The setting agent in step SS004 includes the following raw materials in parts by weight: 8 parts of a color fixing agent, 6 parts of a stabilizer, 3 parts of a fatty alcohol polyoxyethylene ether, and 83 parts of deionized water. The color fixing agent is composed of carrageenan and polydimethyldiallylammonium chloride, and the stabilizer includes polyacrylate.
[0043] SS005, antibacterial treatment, the fabric after shaping is put into the antibacterial composite liquid and allowed to stand, and then the fabric is dehydrated and dried in sequence;
[0044] In step SS005, the antibacterial composite liquid is a mixture of an antibacterial finishing agent and deionized water of polyoxyethylene sorbitan fatty acid ester, the antibacterial finishing agent is chitin, the pH value of the antibacterial composite liquid is 6.6, and the weight percentage of the antibacterial finishing agent in the antibacterial composite liquid is 0.3%;
[0045] SS06, tail treatment, the fabric treated with antibacterial treatment in SS005 is cleaned and dried, and after drying, the fabric is sequentially subjected to shearing, ironing and cutting treatments to obtain double-sided comfortable mini waffle fabric with different styles.
[0046] Embodiment 2
[0047] See also Figure 1-3 The present invention is a weaving method of a double-sided, different-style, comfortable mini waffle fabric:
[0048] SS001, weaving, using a double-sided knitting circular machine for knitting fabrics. The gasket of the lower needle cylinder in the double-sided knitting circular machine is a 120-thread gasket. Through the above-mentioned structural setting, the floating thread coils of the lower needle for 6 consecutive times are stacked neatly and are not hit by the upper needle. The height of the triangular needle pressing point of the floating thread coil of the cylinder needle in the double-sided knitting circular machine is 2mm lower than that of the triangular needle pressing point of the floating thread coil of the traditional cylinder needle. The height of the triangular needle pressing point of the floating thread coil of the cylinder needle is marked as H. Through this structural setting, the quality problems of holes, buckles and anti-spandex yarn on the cloth surface are solved;
[0049] When weaving, the following rules are followed: 14 loops are used as a loop to form the upper and lower sides of the fabric. Spandex yarn is added to the needles of the 1st, 2nd, 3rd, 4th, 5th, and 6th loops, and no spandex yarn is added to the needles of the 7th, 8th, 9th, 10th, 11th, 12th, 13th, and 14th loops. The spandex yarn is 30D spandex, that is, 9000 meters of spandex has a weight of 30 grams;
[0050] Routes 1-14 all use 40s combed cotton blended yarn as raw material.
[0051] The yarn feeding amount of 1, 2, 3, 4, 5, and 6 routes is 425 mm yarn length per 100 needles, and the yarn feeding amount of 7-14 routes is 215 mm yarn length per 100 needles;
[0052] During knitting, the upper layer of the fabric is double-row, and the knitting arrangement of the double-rows in 1, 2, 3, 4, 5, and 6 routes in the upper layer is all loop triangles, and the knitting arrangement of the double-rows in 7, 8, 9, 10, 11, 12, 13, and 14 routes in the upper layer is all floating coils. The lower layer of the fabric is four-row, and in the lower layer, the knitting arrangement of the four-rows in 1, 2, 3, 4, 5, and 6 routes is loop triangle, loop triangle, floating coil, and floating coil from the inside to the outside, the knitting arrangement of the four-rows in 7, 9, 11, and 13 routes is floating coil, loop triangle, floating coil, and loop triangle from the inside to the outside, and the knitting arrangement of the four-rows in 8, 10, 12, and 14 routes is loop triangle, floating coil, loop triangle, and floating coil from the inside to the outside.
[0053] SS002, finishing. After step SS001, the woven grey cloth is obtained. After the weaving of the grey cloth is completed, the grey cloth is immersed in the finishing agent for finishing. After finishing, the raw cloth is obtained. The specific steps of finishing in step SS002 are to soak the grey cloth twice at room temperature, boil it in the working liquid for 3 hours after removing water, and then wash it with 98°C water for 5 times. During the washing process, synchronous stirring operation is performed, the stirring time is 30 minutes, and the stirring times are times. After washing, steam heating is performed for a specified time, and the specified steam heating time is 60 minutes. Drying is performed after steam heating;
[0054] The working solution composition is as follows: sodium hydroxide 5g / L, sodium chloride concentration is .5g / L;
[0055] SS003, degreasing and dyeing, the raw cloth after step SS002 is degreased and dyed in sequence, and then dried at a low temperature within 90°C;
[0056] SS004, shaping, after step SS003, the shaping agent is evenly sprayed on the surface of the fabric treated in step SS003. After the shaping agent is sprayed, it is left to stand for 90 minutes. After standing, the fabric is passed through the shaping machine at a speed of 45 yards. The shaping temperature of the shaping machine is 245°C;
[0057] The setting agent in step SS004 includes the following raw materials in parts by weight: 10 parts of a color fixing agent, 11 parts of a stabilizer, 5 parts of a fatty alcohol polyoxyethylene ether, and 74 parts of deionized water. The color fixing agent is composed of carrageenan and polydimethyldiallylammonium chloride, and the stabilizer includes sodium alginate.
[0058] SS005, antibacterial treatment, the fabric after shaping is put into the antibacterial composite liquid and allowed to stand, and then the fabric is dehydrated and dried in sequence;
[0059] In step SS005, the antibacterial composite liquid is a mixture of an antibacterial finishing agent and deionized water of polyoxyethylene sorbitan fatty acid ester, the antibacterial finishing agent is white mustard oil, the pH value of the antibacterial composite liquid is 6.8, and the weight percentage of the antibacterial finishing agent in the antibacterial composite liquid is 0.55%;
[0060] SS06, tail treatment, the fabric treated with antibacterial treatment in SS005 is cleaned and dried, and after drying, the fabric is sequentially subjected to shearing, ironing and cutting treatments to obtain double-sided comfortable mini waffle fabric with different styles.
[0061] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0062] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A weaving method for double-sided comfortable mini waffle fabric with different styles, characterized in that: The method comprises the following steps: SS001, weaving, use double-sided knitting circular machine to weave the fabric, weave according to the following rules, with 14 routes as a cycle to form the upper and lower sides of the fabric, add spandex yarn to the needles in the 1st, 2nd, 3rd, 4th, 5th and 6th routes, and do not add spandex yarn in the 7th, 8th, 9th, 10th, 11th, 12th, 13th and 14th routes. When weaving, the upper layer of the fabric is double horizontal rows, and the knitting arrangement of the double horizontal rows in the 1st, 2nd, 3rd, 4th, 5th and 6th routes of the upper layer is a loop triangle, and the 7th, 8th, 9th, 10th, 11th, 12th, 13th and 14th routes of the upper layer are all loop triangles. The knitting arrangement of the double rows in the 14-way is all floating coils, and the lower layer of the fabric is four rows. In the lower layer, the knitting arrangement of the four rows in the 1, 2, 3, 4, 5, and 6-way is sequentially looped triangle, looped triangle, floating coil, and floating coil from the inside to the outside, and the knitting arrangement of the four rows in the 7, 9, 11, and 13-way is sequentially floating coil, looped triangle, floating coil, and looped triangle from the inside to the outside, and the knitting arrangement of the four rows in the 8, 10, 12, and 14-way is sequentially looped triangle, floating coil, looped triangle, and floating coil from the inside to the outside; SS002, finishing, after step SS001, the woven grey cloth is obtained. After the weaving of the grey cloth is completed, the grey cloth is immersed in a finishing agent for finishing, and the raw cloth is obtained after finishing; SS003, degreasing and dyeing, the raw cloth after step SS002 is degreased and dyed in sequence, and then dried at a low temperature within 80℃-90℃; SS004, shaping, after step SS003, the shaping agent is evenly sprayed on the surface of the fabric treated in step SS003. After the shaping agent is sprayed, it is left to stand for 70-90 minutes. After standing, the fabric is passed through the shaping machine at a speed of 45 yards. The shaping temperature of the shaping machine is 220℃-245℃; SS005, antibacterial treatment, the fabric after shaping is put into the antibacterial composite liquid and allowed to stand, and then the fabric is dehydrated and dried in sequence; SS006, tail treatment, washing and drying the fabric after antibacterial treatment in SS005, and then performing shearing, ironing and cutting on the fabric in sequence, so as to obtain double-sided comfortable mini waffle fabric with different styles; The yarn feeding amount of the 1st, 2nd, 3rd, 4th, 5th and 6th routes is 425mm yarn length per 100 needles, and the yarn feeding amount of the 7th to 14th routes is 215mm yarn length per 100 needles; The gasket of the lower needle cylinder in the double-sided knitting circular machine is a 120-filament gasket. The height of the triangular needle pressing point of the needle cylinder needle floating line coil in the double-sided knitting circular machine is 2mm lower than the height of the triangular needle pressing point of the needle cylinder needle floating line coil in the traditional needle cylinder needle floating line coil. The height of the triangular needle pressing point of the needle cylinder needle floating line coil is marked as H; The antibacterial composite liquid in the SS005 step is a mixture of an antibacterial finishing agent and deionized water of polyoxyethylene sorbitan fatty acid ester, the pH value of the antibacterial composite liquid is 6.6-6.8, and the weight percentage of the antibacterial finishing agent in the antibacterial composite liquid is 0.3%-0.55%; The setting agent in the SS004 step comprises the following raw materials in parts by weight: 8-10 parts of a color fixing agent, 6-11 parts of a stabilizer, 3-5 parts of a fatty alcohol polyoxyethylene ether, and 74-83 parts of deionized water, wherein the color fixing agent is composed of carrageenan and polydimethyldiallylammonium chloride, and the stabilizer comprises at least one of polyacrylate and sodium alginate; The specific steps of finishing in the SS002 step are to soak the grey cloth twice at room temperature, boil it in the working solution for 1h-3h after removing water, and then wash it with 90℃-98℃ water for 3-5 times. During the washing process, perform synchronous stirring operation, the stirring time is 20min-30min, the stirring frequency is 1-2 times, steam heating is performed for a specified time after washing, and drying is performed after steam heating.
2. The weaving method of a double-sided comfortable mini waffle fabric with different styles according to claim 1, characterized in that: The 1-14 routes all use 40-count combed cotton viscose yarn or blended yarn as raw material, and the spandex yarn uses 30D spandex.
3. The weaving method of a double-sided comfortable mini waffle fabric with different styles according to claim 1, characterized in that: The antibacterial finishing agent is one of chitin, white mustard oil and chitosan or a mixture of two or more thereof.
4. The weaving method of a double-sided comfortable mini waffle fabric with different styles according to claim 1, characterized in that: The working solution is composed of: 15 g / L-25 g / L sodium hydroxide and 0.8 g / L-1.5 g / L sodium chloride.