Amorphous cobalt oxide / carbon / metal organic framework composite material and preparation method and application thereof
By preparing amorphous cobalt oxide/carbon/metal organic frame composite materials, the problems of low specific capacity and poor structural stability of the negative electrode material of lithium-ion batteries are solved, and high specific capacity, long life and excellent cycle stability are achieved, suitable for high Energy density lithium-ion battery.
Patent Information
- Application Number
- CN202211200071.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-09-29
AI Technical Summary
The specific capacity of graphite carbon, the negative electrode material of traditional lithium-ion batteries, is low, which cannot meet the needs of high energy density. At the same time, the volume change of crystalline cobalt oxide during charging and discharging leads to the collapse of the electrode structure, resulting in rapid attenuation of the battery capacity.
Amorphous cobalt oxide/carbon/metal organic frame composite material is used to dissolve cobalt salts and metal heteroatom compounds by ultrasonic dissolution, combined with organic ligands, and heated in a polytetrafluoroethylene reactor, and then calcined at high temperature in an inert atmosphere to form Amorphous cobalt oxide/carbon/metal organic framework composite with high structural stability and active sites.
As the negative electrode material of lithium-ion batteries, this composite material significantly improves cycle life, specific capacity and rate performance, inhibits the collapse of the electrode structure, promotes lithium-ion reaction, and extends the overall life of the battery.
Smart Images

Figure CN115483381B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery technology, and in particular to a preparation method and application of an amorphous cobalt oxide / carbon / metal organic framework composite material. Background Art
[0002] Lithium-ion batteries still occupy a dominant position in the field of energy storage due to their advantages such as high specific energy, long cycle life, high operating voltage and stable operation. They are widely used in various portable electronic devices, various new energy storage power systems, electric vehicles and special aerospace fields. Among them, the negative electrode of lithium-ion batteries, as an important component of the battery, has an important influence on the battery's energy density, rate performance, long cycle life and other performance. Traditional commercial graphite carbon negative electrodes have become increasingly unable to meet people's demand for high energy density lithium-ion batteries due to their low specific capacity. The specific capacity of transition metal cobalt oxide is as high as 700-1000mA hg -1 , has great potential to replace graphite as the next generation of new high-capacity lithium-ion battery negative electrode material. However, the large volume change of crystalline cobalt oxide during the charge and discharge process makes the electrode structure very easy to collapse, ultimately leading to rapid battery capacity decay. Summary of the invention
[0003] In view of this, the present invention provides an amorphous cobalt oxide / carbon / metal organic framework composite material and its preparation method and application. Compared with crystalline cobalt oxide, amorphous cobalt oxide has higher structural stability and more active sites, and its doped metal heteroatoms can further enhance the stability of the material and activate its electrochemical activity. In addition, carbon and metal organic frameworks can also alleviate the structural collapse of the material. Therefore, when the amorphous cobalt oxide / carbon / metal organic framework composite material provided by the present invention is used as an electrode material, it presents the advantages of long life, high specific capacity, excellent cycle stability and rate performance.
[0004] The present invention provides a method for preparing an amorphous cobalt oxide / carbon / metal organic framework composite material, comprising the following steps:
[0005] A certain amount of cobalt salt and a certain amount of metal heteroatom compound are dissolved in a certain amount of organic solution by ultrasonication to obtain solution A;
[0006] A certain amount of organic ligand is dissolved in a certain amount of organic solution by ultrasound to obtain solution B;
[0007] Slowly adding solution B into solution A, stirring for a certain period of time, and then transferring to a polytetrafluoroethylene reactor, heating the reactor to a certain temperature, and keeping the temperature for a certain period of time, and then washing and drying the product to obtain a metal-organic framework precursor;
[0008] The precursor is calcined at high temperature in an inert atmosphere for a certain period of time to obtain an amorphous cobalt oxide / carbon / metal organic framework composite material.
[0009] Furthermore, the cobalt salt is selected from at least one of cobalt nitrate nonahydrate, cobalt chloride and cobalt sulfate;
[0010] The metal heteroatom compound is selected from at least one of iron salt, zinc salt, manganese salt and nickel salt; the iron salt is selected from ferric sulfate heptahydrate, ferric nitrate nonahydrate or ferric chloride, the zinc salt is selected from zinc sulfate heptahydrate, zinc nitrate hexahydrate or zinc chloride, the manganese salt is selected from manganese acetate tetrahydrate or manganese acetate, and the nickel salt is selected from nickel sulfate or nickel chloride.
[0011] The organic ligand is 2-methylimidazole; the organic solution is at least one of methanol, DMF or ethanol.
[0012] Furthermore, in the solution A, the concentration of the cobalt salt is 0.1 mol / L, and the concentration of the metal heteroatom compound is 0.01 to 0.015 mol / L;
[0013] In the solution B, the concentration of the organic ligand is 0.075 mol / L.
[0014] Furthermore, the volume of the organic solution is 40 mL.
[0015] Furthermore, the stirring time after the solution B and the solution A are mixed is 0.5 to 1 h, and the stirring speed is 400 to 500 r / min.
[0016] Furthermore, the insulation temperature of the reactor is 160-200° C., and the insulation time is 36-48 hours.
[0017] Furthermore, the precursor is calcined in an inert atmosphere at a temperature of 400-450° C. for a calcination time of 6-10 hours, and the inert atmosphere is at least one of nitrogen and argon.
[0018] The invention provides an amorphous cobalt oxide / carbon / metal organic framework composite material, and the composite material is prepared by using the above preparation method.
[0019] The present invention also provides a negative electrode, which comprises the amorphous cobalt oxide / carbon / metal organic framework composite material.
[0020] The present invention also provides a lithium ion battery, which comprises the above-mentioned negative electrode.
[0021] Compared with the prior art, the present invention has at least the following beneficial effects:
[0022] The cobalt oxide in the amorphous cobalt oxide / carbon / metal organic framework composite material of the present invention is amorphous cobalt oxide. Compared with crystalline cobalt oxide, the introduction of amorphous cobalt oxide makes the composite material have higher structural stability and more active sites. When the composite material is used as the negative electrode of a lithium ion battery, the collapse of the electrode structure is suppressed and the reaction of lithium ions on the surface and inside of the electrode is promoted. At the same time, the metal heteroatoms doped in the composite material further improve the stability of the electrode and activate its electrochemical activity. In addition, carbon and metal organic frameworks also help to further improve the structural stability of the electrode. Therefore, when the composite material of the present invention is used as an electrode material, the assembled battery as a whole presents the advantages of longer cycle life, higher specific capacity and excellent rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The present invention is a flow chart of the preparation method of the embodiment of the present invention.
[0024] Figure 2 The XRD diagrams of the composite materials prepared in Examples 1 to 4 of the present invention and Comparative Example 1 are shown.
[0025] Figure 3 The SEM images of the composite materials prepared in Examples 1 to 4 of the present invention and Comparative Example 1 are shown.
[0026] Figure 4 The composite materials prepared in Examples 1 to 4 and Comparative Example 1 of the present invention are used for the negative electrode of a lithium ion battery at 1000 mA g -1 Constant current charge and discharge performance diagram under current density.
[0027] Figure 5 The composite materials prepared in Examples 1 to 4 and Comparative Example 1 of the present invention are used for the negative electrode of a lithium ion battery at 2000 mA g -1 Constant current charge and discharge performance diagram under current density. DETAILED DESCRIPTION
[0028] Next, the technical solutions in the embodiments of the present invention will be clearly and completely described in conjunction with the drawings of the present invention. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, other embodiments obtained by ordinary technicians in this field without creative work are all within the scope of protection of the present invention. The experimental methods described in the following embodiments are all conventional methods unless otherwise specified; the reagents and materials, unless otherwise specified, can be obtained from public commercial channels.
[0029] Example 1
[0030] 4mmol of cobalt nitrate nonahydrate and 0.4mmol of ferrous sulfate heptahydrate were dissolved in 40mL of methanol solution by ultrasound to obtain solution A, and 3mmol of 2-methylimidazole was dissolved in 40mL of methanol solution by ultrasound to obtain solution B. Solution B was slowly added to solution A, and stirred for 1h under magnetic stirring at a speed of 400r / min to obtain a mixed solution. The mixed solution was then transferred to a 100mL polytetrafluoroethylene reactor and placed in a drying oven at 160°C for 36h, and then the product was washed and dried to obtain a metal-organic framework precursor;
[0031] The precursor was calcined at 400°C for 6 hours in an inert atmosphere and then cooled naturally in the furnace to finally obtain a Fe-doped amorphous cobalt oxide / carbon / metal organic framework composite material.
[0032] Example 2
[0033] In this embodiment, zinc sulfate heptahydrate is used to replace the iron sulfate heptahydrate in Embodiment 1, and the other conditions are the same as those in Embodiment 1, and finally a metal Zn-doped amorphous cobalt oxide / carbon / metal organic framework composite material is obtained.
[0034] Example 3
[0035] In this embodiment, manganese acetate tetrahydrate is used to replace ferric sulfate heptahydrate in Embodiment 1, and the other conditions are the same as those in Embodiment 1, and finally a metal Mn-doped amorphous cobalt oxide / carbon / metal organic framework composite material is obtained.
[0036] Example 4
[0037] In this embodiment, nickel sulfate is used to replace the ferrous sulfate heptahydrate in Embodiment 1, and the other conditions are the same as those in Embodiment 1, and finally a metal Ni-doped amorphous cobalt oxide / carbon / metal organic framework composite material is obtained.
[0038] Comparative Example 1
[0039] 4mmol of cobalt nitrate nonahydrate and 0.4mmol of copper sulfate pentahydrate were ultrasonically dissolved in 40mL of methanol solution to obtain solution A, and 3mmol of 2-methylimidazole was ultrasonically dissolved in 40mL of methanol solution to obtain solution B. Solution B was slowly added to solution A, and stirred for 1h under magnetic stirring at a speed of 400r / min to obtain a mixed solution. The mixed solution was then transferred to a 100mL polytetrafluoroethylene reactor and placed in a drying oven at 160°C for 36h, and then the product was washed and dried to obtain a metal-organic framework precursor;
[0040] The precursor is calcined at 400°C for 6 hours in an inert atmosphere, and then cooled naturally in the furnace, thereby finally obtaining a Cu-doped crystalline cobalt oxide / carbon / metal organic framework composite material.
[0041] Example 5
[0042] 4mmol of cobalt nitrate nonahydrate and 0.5mmol of ferric chloride were ultrasonically dissolved in 40mL of methanol solution to obtain solution A, and 3mmol of 2-methylimidazole was ultrasonically dissolved in 40mL of methanol solution to obtain solution B. Solution B was slowly added to solution A, and stirred for 1.5h under magnetic stirring at a speed of 450r / min to obtain a mixed solution. The mixed solution was then transferred to a 100mL polytetrafluoroethylene reactor and placed in a drying oven at 180°C for 42h, and then the product was washed and dried to obtain a metal-organic framework precursor;
[0043] The precursor was calcined at 425°C for 8 hours in an inert atmosphere and then cooled naturally in the furnace to finally obtain a metal Fe-doped amorphous cobalt oxide / carbon / metal organic framework composite material.
[0044] Example 6
[0045] 4mmol of cobalt chloride and 0.6mmol of ferric nitrate were dissolved in 40mL of methanol solution by ultrasound to obtain solution A, and 3mmol of 2-methylimidazole was dissolved in 40mL of methanol solution by ultrasound to obtain solution B. Solution B was slowly added to solution A, and stirred for 2h under magnetic stirring at a speed of 500r / min to obtain a mixed solution. The mixed solution was then transferred to a 100mL polytetrafluoroethylene reactor and placed in a drying oven at 200°C for 48h, and then the product was washed and dried to obtain a metal-organic framework precursor;
[0046] The precursor was calcined at 450°C for 10 hours in an inert atmosphere and then cooled naturally in the furnace to finally obtain a Fe-doped amorphous cobalt oxide / carbon / metal organic framework composite material.
[0047] Example 7
[0048] 4mmol of cobalt chloride and 0.4mmol of ferric chloride were dissolved in 40mL of methanol solution by ultrasound to obtain solution A, and 3mmol of 2-methylimidazole was dissolved in 40mL of methanol solution by ultrasound to obtain solution B. Solution B was slowly added to solution A, and stirred for 1h under magnetic stirring at a speed of 400r / min to obtain a mixed solution. The mixed solution was then transferred to a 100mL polytetrafluoroethylene reactor and placed in a drying oven at 160°C for 36h, and then the product was washed and dried to obtain a metal-organic framework precursor;
[0049] The precursor was calcined at 400°C for 6 hours in an inert atmosphere and then cooled naturally in the furnace to finally obtain a Fe-doped amorphous cobalt oxide / carbon / metal organic framework composite material.
[0050] Example 8
[0051] 4mmol of cobalt sulfate and 0.4mmol of ferric chloride were dissolved in 40mL of methanol solution by ultrasound to obtain solution A, and 3mmol of 2-methylimidazole was dissolved in 40mL of methanol solution by ultrasound to obtain solution B. Solution B was slowly added to solution A, and stirred for 1.5h under magnetic stirring at a speed of 450r / min to obtain a mixed solution. The mixed solution was then transferred to a 100mL polytetrafluoroethylene reactor and placed in a drying oven at 180°C for 42h, and then the product was washed and dried to obtain a metal-organic framework precursor;
[0052] The precursor was calcined at 425°C for 8 hours in an inert atmosphere and then cooled naturally in the furnace to finally obtain a Fe-doped amorphous cobalt oxide / carbon / metal organic framework composite material.
[0053] Figure 1 This is a flow chart for preparing a metal heteroatom-doped amorphous cobalt oxide / carbon / metal organic framework composite material according to an embodiment of the present invention.
[0054] Figure 2 The X-ray diffraction patterns (XRD) of the composite materials obtained from Example 1 to Example 4 and Comparative Examples 1 and 2 are shown in Figure (b). Figure (b) is a partial enlarged view of Figure (a). As shown in the figure, when different metal heteroatom compounds are used as raw materials, the diffraction patterns of the corresponding composite materials obtained all have characteristic peaks corresponding to the metal organic framework (ZIF-67) and the carbon phase. Wherein, when the metal heteroatom is copper, the XRD diffraction peaks of crystalline cobalt oxide appear in the diffraction pattern, while when doped with other metal heteroatoms and undoped, the diffraction peaks of cobalt oxide do not appear. Therefore, amorphous cobalt oxide / carbon / metal organic framework composite materials can be obtained when doped with heteroatoms such as iron, manganese, nickel and zinc.
[0055] Figure 3The figures (a1) and (a2) are SEM images of the metal Mn-doped amorphous cobalt oxide / carbon / metal organic framework composite material prepared in Example 3, (b1) and (b2) are SEM images of the metal Cu-doped crystalline cobalt oxide / carbon / metal organic framework composite material prepared in Comparative Example 1, (c1) and (c2) are SEM images of the metal Ni-doped amorphous cobalt oxide / carbon / metal organic framework composite material prepared in Example 4, (d1) and (d2) are SEM images of the metal Zn-doped amorphous cobalt oxide / carbon / metal organic framework composite material prepared in Example 2, (e1) and (e2) are SEM images of the metal Fe-doped amorphous cobalt oxide / carbon / metal organic framework composite material prepared in Example 1, and the figures on the right are partial enlarged figures of the figures on the left. As can be seen from the figure, the prepared composite material is self-assembled by particles of different sizes. When different metal heteroatom compounds are used as raw materials, the final composite material morphology is different. In particular, when zinc sulfate heptahydrate and copper sulfate pentahydrate are used as synthetic raw materials, the composite material obtained is a tremella-like and sea urchin-like microstructure assembled by nanoparticles. This structure significantly increases the specific surface area of the material, shortens the diffusion path of lithium ions, and increases the reactivity of the composite material, thereby greatly improving the specific capacity of the electrode.
[0056] Figure 4 and Figure 5 The electrochemical performance of the cobalt oxide / carbon / metal organic framework composite materials prepared in Examples 1 to 4 of the present invention and Comparative Example 1 when used for the negative electrode of a lithium ion battery is shown. The composite materials prepared in Examples 1 to 4 and Comparative Example 1 are respectively used as the active materials of the negative electrode of a lithium ion battery, and the composite materials, conductive carbon black super P, and adhesive with a mass ratio of 7:2:1 are taken and ground evenly, and then deionized water is added and continued to grind until it is in a paste state, and evenly coated on a copper foil, and dried in a vacuum environment at a temperature of 60°C for a drying time of 12 hours to obtain a negative electrode of a lithium ion battery; the battery is assembled with lithium metal, commercial lithium hexafluorophosphate and a polypropylene separator. Figure 4 The composite materials prepared in Examples 1 to 4 and Comparative Example 1 are used for the negative electrode of lithium ion batteries at 1000 mA g -1 Constant current charge and discharge performance diagram under current density. Figure 5 The composite materials prepared in Examples 1 to 4 and Comparative Example 1 are used for the negative electrode of lithium ion batteries at 2000 mA g -1 The constant current charge and discharge performance diagram under current density. It can be seen from the figure that at 1000mA g -1At the current density, Zn-CoO / NC / ZIF-67 exhibits a high specific capacity and excellent cycle stability. After 500 cycles, its specific capacity is as high as 1000mAh g -1 Although Cu-CoO / NC / ZIF-67 has the highest initial capacity, its first cycle coulombic efficiency is low, and there is obvious capacity decay after 80 cycles. This may be due to the serious structural collapse of crystalline CoO during the charge and discharge process. -1 At current density of 1000 mA g -1 This fully demonstrates that the amorphous cobalt oxide / carbon / metal organic framework composite material obtained by doping with zinc, iron, manganese and nickel heteroatoms of the present invention has higher cycle stability and rate performance.
[0057] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing an amorphous cobalt oxide / carbon / metal organic framework composite material, characterized in that: The following steps are involved: A certain amount of cobalt salt and a certain amount of metal-doped salt are dissolved in a certain amount of organic solution by ultrasonication to obtain solution A; A certain amount of 2-methylimidazole organic ligand was dissolved in 40 ml of organic solution by ultrasonication to obtain solution B; Slowly adding solution B into solution A, stirring for a certain period of time, and then transferring to a polytetrafluoroethylene reactor, heating the reactor to a certain temperature, and keeping the temperature for a certain period of time, and then washing and drying the product to obtain a metal-organic framework precursor; The precursor is calcined at a high temperature for a certain period of time in an inert atmosphere to obtain an amorphous cobalt oxide / carbon / metal organic framework composite material; The cobalt salt is selected from at least one of cobalt nitrate nonahydrate, cobalt chloride and cobalt sulfate; the metal-doped salt is selected from at least one of iron salt, zinc salt, manganese salt and nickel salt; the iron salt is selected from ferrous sulfate heptahydrate, ferric nitrate nonahydrate or ferric chloride, the zinc salt is selected from zinc sulfate heptahydrate, zinc nitrate hexahydrate or zinc chloride, the manganese salt is selected from manganese acetate tetrahydrate, the nickel salt is selected from nickel sulfate or nickel chloride; the organic solution is selected from at least one of methanol, DMF or ethanol; In the solution A, the molar concentration of the cobalt salt is 0.1 mol / L, and the molar concentration of the metal-doped salt is 0.01-0.015 mol / L; in the solution B, the concentration of the organic ligand is 0.075 mol / L; The stirring time after mixing the solution B and the solution A is 0.5-1 h, and the stirring speed is 400-500 r / min; the insulation temperature of the reactor is 160-200° C., and the insulation time is 36-48 h; the temperature of calcining the precursor in an inert atmosphere is 400-450° C., and the calcination time is 6-10 h, and the inert atmosphere is selected from at least one of nitrogen and argon.
2. An amorphous cobalt oxide / carbon / metal organic framework composite material, characterized in that: The preparation method according to claim 1 is used to prepare the product.
3. A negative electrode, characterized in that: The amorphous cobalt oxide / carbon / metal organic framework composite material comprises the amorphous cobalt oxide / carbon / metal organic framework composite material according to claim 2.
4. A lithium ion battery, characterized in that: Comprising the negative electrode of claim 3.