Degradable copolyester and preparation method and product thereof
By introducing hydroxy fatty acids, the ratio of terephthalic acid and aliphatic dibasic acid is regulated, and degradable copolyesters with excellent biodegradation and gas barrier properties are prepared, which solves the problems of low PBAT degradation rate and poor gas barrier properties. Suitable for packaging materials and other fields.
Patent Information
- Application Number
- CN202210982310.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-08-16
AI Technical Summary
Polytetraphthalic acid/butylene adipate (PBAT) has a low degradation rate in natural environment and poor gas barrier properties, making it difficult to meet the market demand for degradable materials.
By introducing hydroxy fatty acids or their esterides, the ratio of terephthalic acid, aliphatic dibasic acid and hydroxy fatty acids is prepared, a degradable copolyester has a crystalline structure and an amorphous regional structure, and improves biodegradable properties and Gas barrier properties and improve mechanical and thermal properties.
It has achieved stable use in the range of -5℃ to 80℃, significantly improved the gas barrier properties and mechanical properties of the degradable copolyester, met the market demand for degradable materials, and is suitable for packaging materials and plastic containers and other products.
Smart Images

Figure CN115490840B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a degradable copolyester and a preparation method and a product thereof. Background Art
[0002] Polybutylene terephthalate / adipate (PBAT) is a highly regarded biodegradable material that can replace non-degradable materials such as polyethylene and polypropylene, effectively alleviating the white pollution problem caused by polymer materials. However, since PBAT needs to be degraded in an environment with a high microbial content such as composting, its degradation rate is low in the natural environment, making it difficult to meet the market demand for degradable materials. In addition, PBAT also has problems such as poor gas barrier properties. Summary of the invention
[0003] Based on this, it is necessary to provide a degradable copolyester and a preparation method thereof to address the above problems. The degradable copolyester not only has excellent biodegradability and natural environmental degradation performance, but also has excellent gas barrier properties, heat resistance and mechanical properties, and can be widely used in the preparation of packaging materials, plastic containers and other products.
[0004] A degradable copolyester, the structural formula of the degradable copolyester is shown in the following formula (1):
[0005]
[0006] In formula (1), R1 and R3 are independently selected from the structural units of ethylene glycol or 1,4-butanediol, R2 is selected from the structural units of aliphatic dibasic acids or their esters, R4 is selected from the structural units of hydroxy fatty acids or their esters, x, y, z, and m are all integers, x=1-10, y=1-10, z=1-10, and m=20-100;
[0007] The sum of the molar amounts of R2 and R4 is The molar ratio of R2 to R4 is 3:2-2:3, and the molar ratio of R2 to R4 is 9:1-1:9.
[0008] In one embodiment, the R4 is selected from a structural unit of a hydroxy fatty acid having 2 to 5 carbon atoms or an ester thereof.
[0009] In one embodiment, the hydroxy fatty acid or its ester is selected from at least one of glycolic acid, esters of glycolic acid, 3-hydroxypropionic acid, esters of 3-hydroxypropionic acid, 4-hydroxybutyric acid, esters of 4-hydroxybutyric acid, lactic acid, and esters of lactic acid.
[0010] In one embodiment, the aliphatic dibasic acid or its ester is selected from at least one of malonic acid, esters of malonic acid, succinic acid, esters of succinic acid, glutaric acid, esters of glutaric acid, adipic acid, esters of adipic acid, suberic acid, esters of suberic acid, azelaic acid, esters of azelaic acid, sebacic acid, and esters of sebacic acid.
[0011] In one embodiment, the intrinsic viscosity of the degradable copolyester is 0.8 dL / g-1.5 dL / g, and the number average molecular weight is 35000 g / mol-60000 g / mol.
[0012] A method for preparing the above-mentioned degradable copolyester comprises the following steps:
[0013] Under a protective atmosphere, a first monomer, a second monomer, and a third monomer are mixed with an esterification catalyst for esterification reaction to obtain a polyester oligomer, wherein the first monomer is selected from terephthalic acid or its esterification product, the second monomer is selected from aliphatic dibasic acid or its esterification product, and the third monomer is selected from ethylene glycol or 1,4-butanediol;
[0014] Under a protective atmosphere, mixing a fourth monomer with a condensation catalyst for condensation reaction to obtain a polyhydroxy fatty acid oligomer, wherein the fourth monomer is selected from a hydroxy fatty acid or an ester thereof;
[0015] Under vacuum conditions, the polyester oligomer, the polyhydroxyalkanoic acid oligomer and a condensation catalyst are mixed to carry out a melt condensation reaction to obtain a degradable copolyester, wherein the ratio of the sum of the molar amounts of the second monomer and the fourth monomer to the molar amount of the first monomer is 3:2-2:3, and the molar ratio of the second monomer to the fourth monomer is 9:1-1:9.
[0016] In one embodiment, the ratio of the sum of the molar amounts of the first monomer and the second monomer to the molar amount of the third monomer is 1:1.2-1:2.0.
[0017] In one embodiment, in the step of mixing the polyester oligomer, the polyhydroxyalkanoic acid oligomer and the polycondensation catalyst for melt polycondensation reaction, a stabilizer is also added.
[0018] In one embodiment, the esterification reaction temperature is 140°C-155°C, and the time is 4h-7h;
[0019] And / or, the condensation reaction temperature is 120°C-180°C, and the time is 5h-10h;
[0020] And / or, the temperature of the melt polycondensation reaction is 180°C-210°C, the time is 5h-10h, and the melt polycondensation reaction is carried out under the condition of vacuum degree less than or equal to 30Pa.
[0021] An article made of the degradable copolyester as described above.
[0022] In the degradable copolyester of the present invention, hydroxy fatty acids or their esters are introduced for copolymerization, and the ratio of terephthalic acid or its esters, aliphatic dibasic acids or their esters and hydroxy fatty acids or their esters is regulated, so that the degradable copolyester has a crystalline structure and an amorphous region structure. This can not only improve the hydrophilicity of the degradable copolyester while maintaining or improving the biodegradability of the degradable copolyester, but also improve the degradation ability of the degradable copolyester in natural environments such as soil and ocean, and is conducive to improving the mechanical properties and thermal properties of the degradable copolyester, so that the degradable copolyester can be stably used in the range of -5°C to 80°C.
[0023] At the same time, the introduction of hydroxy fatty acids or their esters can also reduce the structural proportion of methylene units in the degradable copolyester structure, which is beneficial to enhance the barrier ability of the amorphous region structure in the degradable copolyester to small gas molecules such as CO2, O2, and N2, thereby making the degradable copolyester have excellent gas barrier properties.
[0024] Therefore, the degradable copolyester provided by the present invention can meet the market demand for degradable materials, and can be widely used in products such as cling film, express packaging, food packaging, and food tableware, which is helpful to solve problems such as plastic pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The NMR of the degradable copolyester prepared in Example 1 of the present invention is 1 H-NMR spectrum;
[0026] Figure 2 This is the DSC graph of the degradable copolyester prepared in Example 1 of the present invention;
[0027] Figure 3 This is the stress-strain diagram of the degradable copolyester prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0028] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific implementation methods or embodiments and are not intended to limit the present invention.
[0030] The present invention provides a degradable copolyester, the structural formula of the degradable copolyester is shown in the following formula (1):
[0031]
[0032] In formula (1), R1 and R3 are independently selected from the structural units of ethylene glycol or 1,4-butanediol, R2 is selected from the structural units of aliphatic dibasic acids or their esters, R4 is selected from the structural units of hydroxy fatty acids or their esters, x, y, z, and m are all integers, x=1-10, y=1-10, z=1-10, and m=20-100;
[0033] The sum of the molar amounts of R2 and R4 is The molar ratio of R2 to R4 is 3:2-2:3, and the molar ratio of R2 to R4 is 9:1-1:9.
[0034] It should be noted that the R1 or R3 structural unit is -O-(CH2)2-O- or -O-(CH2)4-O- obtained by removing -H from the hydroxyl group of ethylene glycol or 1,4-butanediol in an esterification reaction; R2 is -OC-R2-CO- obtained by removing -OH from the carboxyl group of an aliphatic dibasic acid or its esterify (HOOC-R2-COOH) in an esterification reaction; R4 is -O-R4-CO- obtained by removing -H from the hydroxyl group and -OH from the carboxyl group of a hydroxy fatty acid or its esterify (HO-R4-COOH) in a condensation reaction.
[0035] In the polyester structure, the amorphous region structure dominated by aliphatic dibasic acid segments is the main segment area for small gas molecules such as CO2, O2, and N2 to diffuse through the polyester. The higher the proportion of methylene in the dibasic acid, the worse the gas barrier performance of the polyester. In the traditional polybutylene terephthalate / adipate (PBAT) molecular structure, 53%-55% of the dibasic acid is adipic acid, which leads to poor gas barrier performance of PBAT.
[0036] In the degradable copolyester provided by the present invention, the introduction of hydroxy fatty acid or its esterified product structural unit can, on the one hand, reduce the structural proportion of methylene units in the structure of the degradable copolyester, which is beneficial to enhance the barrier ability of the amorphous region structure in the degradable copolyester to small gas molecules such as CO2, O2, N2, so that the degradable copolyester has excellent gas barrier properties; on the other hand, it is beneficial to improve the hydrophilicity of the degradable copolyester, so that the degradable copolyester can not only meet the requirements of biodegradability, but also improve the degradation ability of the degradable copolyester in natural environments such as soil and ocean.
[0037] In one embodiment, the R4 is preferably a structural unit of a hydroxy fatty acid having 2 to 5 carbon atoms or an ester thereof.
[0038] Specifically, the hydroxy fatty acid or its ester is selected from at least one of glycolic acid, esters of glycolic acid, 3-hydroxypropionic acid, esters of 3-hydroxypropionic acid, 4-hydroxybutyric acid, esters of 4-hydroxybutyric acid, lactic acid, and esters of lactic acid.
[0039] By adjusting the ratio of the structural unit of the aliphatic dibasic acid or its ester and the structural unit of the hydroxy fatty acid or its ester, a degradable copolyester with a lower glass transition temperature can be obtained, which is beneficial to improve the low temperature resistance of the degradable copolyester. Specifically, when the molar ratio of the structural unit of the aliphatic dibasic acid or its ester to the structural unit of the hydroxy fatty acid or its ester is 9:1-1:9, the glass transition temperature of the degradable copolyester ranges from -30°C to -5°C, so that the degradable copolyester has stability in use under low temperature conditions.
[0040] Furthermore, in the structural formula of the degradable copolyester, the molar ratio of R2 to R4 is preferably 1:4-4:1.
[0041] Specifically, the aliphatic dibasic acid or its ester is selected from at least one of malonic acid, esters of malonic acid, succinic acid, esters of succinic acid, glutaric acid, esters of glutaric acid, adipic acid, esters of adipic acid, suberic acid, esters of suberic acid, azelaic acid, esters of azelaic acid, sebacic acid, and esters of sebacic acid.
[0042] By precisely controlling the ratio of terephthalic acid or its ester structural unit, aliphatic dibasic acid or its ester structural unit and hydroxy fatty acid or its ester structural unit in the degradable copolyester, on the one hand, the content of terephthalic acid or its ester structural segment can be maintained at 40%-60%, so that the degradable copolyester has a stable crystal structure and crystallization ability, and the overall crystallization rate and melting point of the degradable copolyester are improved, which is beneficial to improve the heat resistance temperature of the degradable copolyester. Specifically, the melting temperature range of the degradable copolyester of the present invention is 90°C-150°C, and the fastest half crystallization time is 90 seconds-180 seconds, so that the degradable copolyester has an upper limit of use temperature of up to 50°C-80°C; on the other hand, compared with traditional PBAT and other biodegradable materials, the mechanical properties of the degradable copolyester in strength, modulus, elongation at break, etc. can be significantly improved, which is beneficial to expand the application field of the degradable copolyester.
[0043] Further, in the structural formula of the degradable copolyester, the sum of the molar amounts of R2 and R4 is The molar ratio of is preferably 3:2-5:5.
[0044] In one embodiment, the degradable copolyester has a higher intrinsic viscosity, specifically, the intrinsic viscosity is 0.8dL / g-1.5dL / g, preferably 1.0dL / g-1.4dL / g; the degradable copolyester also has a higher molecular weight, specifically, the number average molecular weight is 35000g / mol-60000g / mol, preferably 40000g / mol-60000g / mol.
[0045] Therefore, the degradable copolyester of the present invention not only has excellent biodegradability and natural environment degradation performance, but also has good mechanical and thermal properties, so that the degradable copolyester can be stably used in the range of -5°C to 80°C. At the same time, the degradable copolyester also has excellent gas barrier properties and can effectively block small gas molecules such as CO2, O2, and N2.
[0046] In one embodiment, the structural formula of the degradable copolyester is preferably as shown in the following formula (1-1), formula (1-2), formula (1-3), and formula (1-4):
[0047]
[0048] Among them, x, y, z, and m are all integers, x=1-10, y=1-10, z=1-10, and m=20-100.
[0049] The present invention also provides a method for preparing the degradable copolyester, comprising the following steps:
[0050] S1, under a protective atmosphere, mixing a first monomer, a second monomer, and a third monomer with an esterification catalyst for esterification reaction to obtain a polyester oligomer, wherein the first monomer is selected from terephthalic acid or its esterification product, the second monomer is selected from aliphatic dibasic acid or its esterification product, and the third monomer is selected from ethylene glycol or 1,4-butanediol;
[0051] S2, under a protective atmosphere, mixing a fourth monomer with a condensation catalyst for condensation reaction to obtain a polyhydroxy fatty acid oligomer, wherein the fourth monomer is selected from a hydroxy fatty acid or an ester thereof;
[0052] S3, under vacuum conditions, mixing the polyester oligomer, the polyhydroxyalkanoic acid oligomer and a condensation catalyst for melt condensation reaction to obtain a degradable copolyester, wherein the ratio of the sum of the molar amounts of the second monomer and the fourth monomer to the molar amount of the first monomer is 3:2-2:3, and the molar ratio of the second monomer to the fourth monomer is 9:1-1:9.
[0053] In step S1, the structural formula of the polyester oligomer is Wherein, R1 and R3 are independently selected from the structural units of the third monomer, R2 is selected from the structural units of the second monomer, and p, q, and n are all integers, p=1-3, q=1-3, and n=1-3.
[0054] In order to control the structure of the polyester oligomer, the ratio of the sum of the molar amounts of the first monomer and the second monomer to the molar amount of the third monomer is selected to be 1:1.2-1:2.0.
[0055] In one embodiment, the mass of the esterification catalyst is 2‰-6‰ of the total mass of the first monomer, the second monomer, the third monomer and the fourth monomer.
[0056] Specifically, the esterification catalyst is selected from at least one of a titanium-based catalyst, an antimony-based catalyst, and a tin-based catalyst, preferably at least one of tetrabutyl titanate, isopropyl titanate, and antimony acetate.
[0057] In one embodiment, the esterification reaction is carried out at a temperature of 140° C. to 155° C. and for a time of 4 h to 7 h.
[0058] In step S2, the structural formula of the polyhydroxyalkanoic acid oligomer is Wherein, R4 is selected from the structural unit of the fourth monomer, g is an integer, and g=5-30.
[0059] In order to precisely control the amount of the introduced structural unit of the hydroxy fatty acid or its ester, the self-polymerization of the hydroxy fatty acid or its ester is utilized to form a polyhydroxy fatty acid oligomer.
[0060] In one embodiment, the mass of the condensation catalyst is 5‰-10‰ of the total mass of the first monomer, the second monomer, the third monomer and the fourth monomer.
[0061] Specifically, the condensation catalyst is selected from at least one of a zinc-based catalyst and a tin-based catalyst, preferably zinc acetate and dibutyltin oxide.
[0062] In one embodiment, the condensation reaction is carried out at a temperature of 120° C. to 180° C. and for a time of 5 h to 10 h.
[0063] It should be noted that there is no particular order for step S1 and step S2. Step S1 may be performed first and then step S2, or step S2 may be performed first and then step S1. Step S1 and step S2 may also be performed simultaneously, and the present invention is not limited to this.
[0064] In step S3, the mass of the condensation catalyst is 5‰-10‰ of the total mass of the first monomer, the second monomer, the third monomer and the fourth monomer, and the condensation catalyst is selected from at least one of a zinc-based catalyst and a titanium-based catalyst, preferably at least one of zinc acetate, tetrabutyl titanate and isopropyl titanate.
[0065] In the step of mixing the polyester oligomer, the polyhydroxyalkanoic acid oligomer and the condensation catalyst for melt polycondensation reaction, a stabilizer is also added, the mass of the stabilizer is 10‰-20‰ of the total mass of the first monomer, the second monomer, the third monomer and the fourth monomer, and the stabilizer is selected from phosphorus stabilizers, wherein the phosphorus stabilizer includes at least one of phosphorous acid, diphenyl phosphate, triphenyl phosphate and triphenyl phosphite, preferably at least one of triphenyl phosphate and triphenyl phosphite.
[0066] In one embodiment, the temperature of the melt polycondensation reaction is 180° C.-210° C., the time is 5 h-10 h, and the melt polycondensation reaction is carried out under a vacuum degree less than or equal to 30 Pa.
[0067] The degradable copolyester of the present invention is prepared by oligomer preparation-polycondensation process, which can not only obtain high molecular weight degradable copolyester, but also has simple preparation method, easy operation, strong controllability, easy implementation, and is suitable for large-scale industrial production.
[0068] The invention also provides a product made of the degradable copolyester.
[0069] The degradable copolyester provided by the present invention can achieve rapid degradation in terrestrial and aquatic environments, can meet the market demand for degradable materials, and can be widely used in products such as cling film, express packaging, food packaging, and food tableware, thereby helping to solve problems such as plastic pollution.
[0070] In one embodiment, the article may be a degradable copolyester film.
[0071] Specifically, the preparation method of the degradable copolyester film includes: vacuum drying the degradable copolyester and then inputting it into a twin-screw extruder, melt-extruded at 150°C-160°C, the melt conveying temperature is 155°C-165°C, and the molten fluid is cast onto a rotating cooling cylinder to obtain a cast thick sheet with a thickness of 1mm-5mm; preheating the cast thick sheet to 80°C-100°C and then stretching it longitudinally by 3 times to 4 times, and then preheating it here and stretching it transversely by 3 times to 5 times to obtain a degradable copolyester film.
[0072] Hereinafter, the degradable copolyester and its preparation method and product will be further described through the following specific examples.
[0073] In the embodiment, the nuclear magnetic resonance spectroscopy 1 H-NMR was measured on a Bruker 400AVANCEⅢ Spectrometer at 400 MHz, with deuterated chloroform (CDCl3) as the solvent.
[0074] In the examples, thermal analysis was performed using differential scanning calorimetry (Mettler Toledo DSC) at a heating rate of 10°C / min in a N2 atmosphere in the temperature range of -60°C to 200°C.
[0075] In the examples, thermogravimetric analysis (TGA) was performed on a Perkin-Elmer Diamond TG / DTA at a heating rate of 20°C / min in a temperature range of 50°C-800°C.
[0076] In the embodiment, the mechanical property test was conducted using an Instron 5567 universal material testing machine, with the sample strip dimensions of 35.0 mm in length, 2.0 mm in width, and 1.0 mm in thickness, and a tensile speed of 20 mm / min.
[0077] In the embodiment, Labthink VAC-V2 was used to test the barrier performance of O2 and CO2, wherein O2 and CO2 were used as gas sources, respectively, and the measurement was carried out under the conditions of temperature of 23°C and humidity of 50% RH. The sample size was Φ=97mm and the permeation area was 38.5cm 2 .
[0078] In the embodiment, a phosphate buffer solution is used as a degradation solvent, and a hydrolysis degradation test is performed at a constant temperature of 37° C., wherein the sample is 10 mm in length, 10 mm in width, and 1.0 mm in thickness.
[0079] In the example, a phosphate buffer solution of 0.1 mg / mL lipase was used as a degradation solvent, and an enzyme degradation test was performed at a constant temperature of 37° C., wherein the sample was 10 mm in length, 10 mm in width, and 1.0 mm in thickness.
[0080] Example 1
[0081] Terephthalic acid, adipic acid and 1,4-butanediol were added into the reactor in molar amounts of 0.5 mol, 0.3 mol and 0.96 mol, respectively, and then zinc acetate (accounting for 4‰ of the total mass of all acid and alcohol raw materials) was added as an esterification catalyst. Under nitrogen protection, the temperature was gradually raised from 140°C to 155°C for esterification, and polyester oligomers were obtained after reacting for 5 hours.
[0082] 0.24 mol of glycolic acid was added into the reactor, and condensation catalyst zinc acetate (accounting for 7‰ of the total mass of all acid and alcohol raw materials) was added. Under nitrogen protection, the condensation temperature was gradually increased from 120°C to 150°C. After reacting for 7 hours, polyglycolic acid oligomers were obtained.
[0083] The polyester oligomer and polyglycolic acid oligomer are mixed, and then a polycondensation catalyst tetrabutyl titanate (accounting for 6.5‰ of the total mass of all acid and alcohol raw materials) and a stabilizer triphenyl phosphate (accounting for 15‰ of the total mass of all acid and alcohol raw materials) are added, and the temperature is gradually increased to 200°C, and the vacuum degree is gradually reduced to 20Pa. The reaction is carried out for 7 hours to obtain a degradable copolyester, whose structural formula is shown in formula (1-1).
[0084]
[0085] Among them, x, y, z, and m are all integers, x=1-10, y=1-10, z=1-10, and m=20-100.
[0086] The NMR of the degradable copolyester prepared in this example 1 H-NMR Figure 1 As shown, the structure of the obtained degradable copolyester is clear; the DSC curve is as follows Figure 2 As shown by Figure 2 It can be seen that the glass transition temperature of the degradable copolyester is -14°C and the melting point is 138°C; the stress-strain curve is as follows Figure 3 As shown by Figure 3 It can be seen that the tensile strength of the degradable copolyester is 26 MPa and the elongation at break is 900%.
[0087] The test results show that the biodegradable copolyester prepared in this embodiment has an intrinsic viscosity of 1.35 dL / g, a number average molecular weight of 41200 g / mol, and a thermal weight loss of T 5% The temperature is 358℃, the elastic modulus is 120MPa, the tensile strength is 26MPa, the elongation at break is 900%, and the water contact angle of the film is 70°. The CO2 permeability is 0.31barrer, and the CO2 barrier performance is 19.0 times that of PBAT; the O2 permeability is 0.045barrer, and the O2 barrier performance is 16.9 times that of PBAT.
[0088] According to tests, the degradable copolyester prepared in this example has a mass loss of 22% after 180 days of degradation in phosphate buffer, a mass loss of 31% after 180 days of degradation in lipase solution, and a weight average molecular weight decrease rate of 72% after 12 months in a marine environment.
[0089] Example 2
[0090] Terephthalic acid, adipic acid and 1,4-butanediol were added into the reactor in molar amounts of 0.5 mol, 0.2 mol and 0.84 mol, and then tetrabutyl titanate (accounting for 5‰ of the total mass of all acid and alcohol raw materials) was added as an esterification catalyst. Under nitrogen protection, the temperature was gradually raised from 140°C to 150°C for esterification, and polyester oligomers were obtained after the reaction for 5.5 hours.
[0091] 0.35 mol of glycolic acid was added into the reactor, and the condensation catalyst dibutyltin oxide (accounting for 6‰ of the total mass of all acid and alcohol raw materials) was added. Under nitrogen protection, the condensation temperature was gradually increased from 130°C to 150°C. After reacting for 6.5 hours, polyglycolic acid oligomers were obtained.
[0092] The polyester oligomer and polyglycolic acid oligomer are mixed, and then polycondensation catalysts tetrabutyl titanate and isopropyl titanate (accounting for 7‰ of the total mass of all acid and alcohol raw materials) and stabilizer triphenyl phosphite (accounting for 20‰ of the total mass of all acid and alcohol raw materials) are added, and the temperature is gradually increased to 185°C, and the vacuum degree is gradually reduced to 15Pa. The reaction is carried out for 8 hours to obtain a degradable copolyester, whose structural formula is shown in formula (1-1).
[0093]
[0094] Among them, x, y, z, and m are all integers, x=1-10, y=1-10, z=1-10, and m=20-100.
[0095] After testing, the biodegradable copolyester prepared in this embodiment has an intrinsic viscosity of 1.27 dL / g, a number average molecular weight of 40500 g / mol, a glass transition temperature of -8°C, a melting point of 131°C, and a thermal weight loss of 0.1%. 5%The temperature is 361℃, the elastic modulus is 145MPa, the tensile strength is 27MPa, the elongation at break is 750%, and the water contact angle of the film is 68°. The CO2 permeability is 0.074barrer, and the CO2 barrier performance is 86 times that of PBAT; the O2 permeability is 0.016barrer, and the O2 barrier performance is 47 times that of PBAT.
[0096] According to tests, the degradable copolyester obtained in this example has a mass loss of 26% after 180 days of degradation in phosphate buffer, a mass loss of 33% after 180 days of degradation in lipase solution, and a weight average molecular weight decrease rate of 81% after 12 months in a marine environment.
[0097] Example 3
[0098] Terephthalic acid, adipic acid and 1,4-butanediol were added into the reactor in molar amounts of 0.5 mol, 0.4 mol and 1.08 mol, and then tetrabutyl titanate (accounting for 6‰ of the total mass of all acid and alcohol raw materials) was added as an esterification catalyst. Under nitrogen protection, the temperature was gradually raised from 130°C to 155°C for esterification, and polyester oligomers were obtained after reacting for 6 hours.
[0099] 0.12 mol of glycolic acid was added to the reactor, and a composite catalyst of dibutyltin oxide and zinc acetate was added (the mass ratio of dibutyltin oxide to zinc acetate was 2:1, and the mass of dibutyltin oxide and zinc acetate accounted for 7‰ of the total mass of all acid and alcohol raw materials). Under nitrogen protection, the condensation temperature was gradually increased from 130°C to 145°C, and the reaction was carried out for 5.5 hours to obtain polyglycolic acid oligomers.
[0100] The polyester oligomer and polyglycolic acid oligomer are mixed, and then a polycondensation catalyst tetrabutyl titanate (accounting for 7‰ of the total mass of all acid and alcohol raw materials) and a stabilizer triphenyl phosphate (accounting for 18‰ of the total mass of all acid and alcohol raw materials) are added, and the temperature is gradually increased to 205°C, and the vacuum degree is gradually reduced to 15Pa. The reaction is carried out for 6 hours to obtain a degradable copolyester, whose structural formula is shown in formula (1-1).
[0101]
[0102] Among them, x, y, z, and m are all integers, x=1-10, y=1-10, z=1-10, and m=20-100.
[0103] The test results show that the biodegradable copolyester prepared in this embodiment has an intrinsic viscosity of 1.18 dL / g, a number average molecular weight of 37600 g / mol, a glass transition temperature of -27°C, a melting point of 130°C, and a thermal weight loss of 0.147 g / mol. 5%The temperature is 360℃, the elastic modulus is 107MPa, the tensile strength is 26.5MPa, the elongation at break is 910%, and the water contact angle of the film is 81°. The CO2 permeability is 0.75barrer, and the CO2 barrier performance is 7.9 times that of PBAT; the O2 permeability is 0.073barrer, and the O2 barrier performance is 10.4 times that of PBAT.
[0104] According to tests, the degradable copolyester prepared in this example has a mass loss of 13.3% after 180 days of degradation in phosphate buffer, a mass loss of 17.5% after 180 days of degradation in lipase solution, and a weight average molecular weight decrease rate of 27.5% after 12 months in a marine environment.
[0105] Example 4
[0106] Terephthalic acid, adipic acid, ethylene glycol and 1,4-butanediol were added into the reactor in molar amounts of 0.5 mol, 0.3 mol, 0.3 mol and 0.6 mol respectively, and then the esterification catalyst tetrabutyl titanate (accounting for 7‰ of the total mass of all acid and alcohol raw materials) was added. Under nitrogen protection, the temperature was gradually raised from 150°C to 155°C for esterification, and polyester oligomers were obtained after the reaction for 6.5 hours.
[0107] 0.25 mol of glycolic acid was added into the reactor, and the condensation catalyst zinc acetate (accounting for 6.5‰ of the total mass of all acid and alcohol raw materials) was added. Under nitrogen protection, the condensation temperature was gradually increased from 140°C to 160°C. After reacting for 5 hours, polyglycolic acid oligomers were obtained.
[0108] The polyester oligomer and polyglycolic acid oligomer are mixed, and then a polycondensation catalyst tetrabutyl titanate (accounting for 7.5‰ of the total mass of all acid and alcohol raw materials) and a stabilizer triphenyl phosphite (accounting for 15‰ of the total mass of all acid and alcohol raw materials) are added, and the temperature is gradually increased to 210°C, and the vacuum degree is gradually reduced to 10Pa. The reaction is carried out for 7 hours to obtain a degradable copolyester, whose structural formula is shown in formula (1-2).
[0109]
[0110] Among them, x, y, z, and m are all integers, x=1-10, y=1-10, z=1-10, and m=20-100.
[0111] The test results show that the biodegradable copolyester prepared in this embodiment has an intrinsic viscosity of 1.02 dL / g, a number average molecular weight of 35200 g / mol, a glass transition temperature of -11°C, a melting point of 98°C, and a thermal weight loss of 0.1447 W / L. 5%The temperature is 340℃, the elastic modulus is 97MPa, the tensile strength is 17.5MPa, the elongation at break is 1050%, and the water contact angle of the film is 82°. The CO2 permeability is 0.25barrer, and the CO2 barrier performance is 23.5 times that of PBAT; the O2 permeability is 0.044barrer, and the O2 barrier performance is 17.2 times that of PBAT.
[0112] According to tests, the degradable copolyester prepared in this example has a mass loss of 20.8% after 180 days of degradation in phosphate buffer, a mass loss of 26.2% after 180 days of degradation in lipase solution, and a weight average molecular weight decrease rate of 51.5% after 12 months in a marine environment.
[0113] Example 5
[0114] Terephthalic acid, succinic acid and ethylene glycol were added into the reactor in molar amounts of 0.5 mol, 0.2 mol and 0.85 mol, respectively, and then a complex of dibutyltin oxide and antimony acetate (accounting for 8‰ of the total mass of all acid and alcohol raw materials) was added as an esterification catalyst. Under nitrogen protection, the temperature was gradually raised from 150°C to 155°C for esterification, and polyester oligomers were obtained after reacting for 6 hours.
[0115] 0.37 mol of 3-hydroxypropionic acid was added into the reactor, and the condensation catalyst dibutyltin oxide (accounting for 5‰ of the total mass of all acid and alcohol raw materials) was used. Under nitrogen protection, the condensation temperature was gradually increased from 140°C to 150°C. After reacting for 5 hours, poly 3-hydroxypropionic acid oligomer was obtained.
[0116] The polyester oligomer and the poly 3-hydroxypropionic acid oligomer are mixed, and then a polycondensation catalyst tetrabutyl titanate and zinc acetate (accounting for 8‰ of the total mass of all acid and alcohol raw materials) and a stabilizer triphenyl phosphite (accounting for 18‰ of the total mass of all acid and alcohol raw materials) are added, and the temperature is gradually increased to 200°C, and the vacuum degree is gradually reduced to 15Pa. The reaction is carried out for 8 hours to obtain a degradable copolyester, whose structural formula is shown in formula (1-3).
[0117]
[0118] Among them, x, y, z, and m are all integers, x=1-10, y=1-10, z=1-10, and m=20-100.
[0119] The test results show that the biodegradable copolyester prepared in this embodiment has an intrinsic viscosity of 1.11 dL / g, a number average molecular weight of 39100 g / mol, a glass transition temperature of -15°C, a melting point of 107°C, and a thermal weight loss of 0.1447 W / L. 5%The temperature is 345℃, the elastic modulus is 133MPa, the tensile strength is 23MPa, the elongation at break is 750%, and the water contact angle of the film is 78°. The CO2 permeability is 0.21barrer, and the CO2 barrier performance is 27.5 times that of PBAT; the O2 permeability is 0.036barrer, and the O2 barrier performance is 21.1 times that of PBAT.
[0120] According to tests, the degradable copolyester prepared in this example has a mass loss of 15.2% after 180 days of degradation in phosphate buffer, a mass loss of 22.2% after 180 days of degradation in lipase solution, and a weight average molecular weight decrease rate of 15.5% after 12 months in a marine environment.
[0121] Example 6
[0122] Terephthalic acid, succinic acid and ethylene glycol were added into the reactor in molar amounts of 0.5 mol, 0.4 mol and 1.05 mol respectively, and then dibutyltin oxide (accounting for 8‰ of the total mass of all acid and alcohol raw materials) was added as an esterification catalyst. Under nitrogen protection, the temperature was gradually raised from 145°C to 155°C for esterification, and polyester oligomers were obtained after 7 hours of reaction.
[0123] 0.24 mol of lactic acid was added into the reactor, and condensation catalyst zinc acetate (accounting for 6‰ of the total mass of all acid and alcohol raw materials) was added. Under nitrogen protection, the condensation temperature was gradually increased from 140°C to 150°C. After reacting for 5 hours, polylactic acid oligomer was obtained.
[0124] The polyester oligomer and the polylactic acid oligomer are mixed, and then polycondensation catalysts tetrabutyl titanate and isopropyl titanate (accounting for 8‰ of the total mass of all acid and alcohol raw materials) and stabilizer triphenyl phosphite (accounting for 18‰ of the total mass of all acid and alcohol raw materials) are added, and the temperature is gradually increased to 200°C, and the vacuum degree is gradually reduced to 15Pa. The reaction is carried out for 8 hours to obtain a degradable copolyester, whose structure is shown in formula (1-4).
[0125]
[0126] Among them, x, y, z, and m are all integers, x=1-10, y=1-10, z=1-10, and m=20-100.
[0127] The test results show that the biodegradable copolyester prepared in this embodiment has an intrinsic viscosity of 0.98 dL / g, a number average molecular weight of 35000 g / mol, a glass transition temperature of -2.8°C, a melting point of 115°C, and a thermal weight loss of 0.1477 W / L. 5%The temperature is 360℃, the elastic modulus is 270MPa, the tensile strength is 27.5MPa, the elongation at break is 378%, and the water contact angle of the film is 80°. The CO2 permeability is 0.29barrer, and the CO2 barrier performance is 20.5 times that of PBAT; the O2 permeability is 0.043barrer, and the O2 barrier performance is 17.5 times that of PBAT.
[0128] According to tests, the degradable copolyester prepared in this example has a mass loss of 22.5% after 180 days of degradation in phosphate buffer, a mass loss of 37.8% after 180 days of degradation in lipase solution, and a weight average molecular weight decrease rate of 27.5% after 12 months in a marine environment.
[0129] Comparative Example 1
[0130] Terephthalic acid, adipic acid and 1,4-butanediol were added into the reactor in molar amounts of 0.55 mol, 0.45 mol and 1.2 mol respectively, and then the esterification catalyst tetrabutyl titanate (accounting for 8‰ of the total mass of all acid and alcohol raw materials) was added. Under nitrogen protection, the temperature was gradually raised from 145°C to 160°C for esterification, and polyester oligomers were obtained after the reaction for 7 hours.
[0131] Then, a mixture of condensation catalysts tetrabutyl titanate and isopropyl titanate (accounting for 7‰ of the total mass of all acid and alcohol raw materials) and a stabilizer triphenyl phosphite (accounting for 20‰ of the total mass of all acid and alcohol raw materials) were added, the temperature was gradually raised to 210°C, the vacuum degree was gradually reduced to 15 Pa, and the reaction was carried out for 8 hours to obtain a degradable polyester whose structure was commercial PBAT.
[0132] After testing, the commercial PBAT prepared in this comparative example has an intrinsic viscosity of 1.20 dL / g, a number average molecular weight of 38200 g / mol, a glass transition temperature of -30°C, a melting point of 125°C, and a thermal weight loss of T 5% The temperature is 360℃, the elastic modulus is 100MPa, the tensile strength is 17.0MPa, the elongation at break is 750%, and the water contact angle of the film is 85°. The permeability of CO2 is 5.9barrer, and the permeability of O2 is 0.076barrer.
[0133] After testing, the commercial PBAT prepared in this comparative example had a mass loss of 5.2% after 180 days of degradation in phosphate buffer, a mass loss of 10.8% after 180 days of degradation in lipase solution, and a weight average molecular weight decrease rate of 7.5% after 12 months in a marine environment.
[0134] Comparative Example 2
[0135] Terephthalic acid, adipic acid, 1,4-butanediol and glycolic acid were added into the reactor in molar amounts of 0.5 mol, 0.3 mol, 0.96 mol and 0.24 mol, and then zinc acetate (accounting for 4‰ of the total mass of all acid and alcohol raw materials) was added as an esterification catalyst. Under nitrogen protection, the temperature was gradually raised from 140°C to 155°C for esterification, and polyester oligomers were obtained after reacting for 5 hours.
[0136] Then add the condensation catalyst tetrabutyl titanate (accounting for 6.5‰ of the total mass of all acid and alcohol raw materials) and the stabilizer triphenyl phosphate (accounting for 15‰ of the total mass of all acid and alcohol raw materials), gradually increase the temperature to 210°C, gradually reduce the vacuum degree to 20Pa, react for 7h, and obtain degradable polyester.
[0137] After testing, the intrinsic viscosity of the biodegradable polyester prepared in this comparative example is 1.05 dL / g, the number average molecular weight is 28700 g / mol, the glass transition temperature is 3.5°C, the melting point is 145°C, and the thermal weight loss T 5% The temperature is 360℃, the elastic modulus is 155.8MPa, the tensile strength is 21.0MPa, the elongation at break is 127%, and the water contact angle of the film is 87°. The CO2 permeability is 1.01barrer, and the CO2 barrier performance is 5.8 times that of PBAT; the O2 permeability is 0.23barrer, and the O2 barrier performance is 3.2 times that of PBAT.
[0138] After testing, the degradable polyester prepared in this comparative example had a mass loss of 2.5% after 180 days of degradation in phosphate buffer, a mass loss of 3.7% after 180 days of degradation in lipase solution, and a weight average molecular weight decrease rate of 1.5% after 12 months in a marine environment.
[0139] Comparative Example 3
[0140] The difference between Comparative Example 3 and Example 1 is that 0.4 mol of terephthalic acid is used instead of 0.5 mol of terephthalic acid, 0.36 mol of adipic acid is used instead of 0.3 mol of adipic acid, and 0.28 mol of glycolic acid is used instead of 0.24 mol of glycolic acid.
[0141] After testing, the intrinsic viscosity of the biodegradable copolyester prepared in this comparative example is 1.17 dL / g, the number average molecular weight is 37600 g / mol, the glass transition temperature is -17.5°C, the melting point is 58.5°C, and the thermal weight loss T 5%The temperature is 317.5℃, the elastic modulus is 17.5MPa, the tensile strength is 7.2MPa, the elongation at break is 620%, and the water contact angle of the film is 57.5°. The CO2 permeability is 3.93barrer, and the CO2 barrier performance is 1.5 times that of PBAT; the O2 permeability is 0.69barrer, and the O2 barrier performance is 1.1 times that of PBAT.
[0142] According to tests, the degradable copolyester prepared in this comparative example had a mass loss of 27% after 180 days of degradation in phosphate buffer, a mass loss of 45% after 180 days of degradation in lipase solution, and a weight average molecular weight decrease rate of 85% after 12 months in a marine environment.
[0143] According to Comparative Example 1, the degradation rate of commercial PBAT structure in marine environment and phosphate buffer is very slow. In Comparative Example 2, glycolic acid is directly mixed with terephthalic acid, adipic acid and 1,4-butanediol for esterification. Based on the low boiling point characteristics of glycolic acid, most of the glycolic acid sublimates in the esterification stage, and the purged nitrogen is blown out of the system, resulting in very little glycolic acid structure entering the copolyester, and thus the degradation effect and barrier performance of the obtained copolyester are not as good as those in Example 1. In Comparative Example 3, due to the excessive amount of adipic acid and glycolic acid introduced, the molar amount of terephthalic acid structural units in the degradable copolymer is low, which makes the mechanical properties and thermal properties of the degradable copolymer not as good as those in Example 1.
[0144] After the present invention introduces hydroxy fatty acids or their esterified structural monomers such as glycolic acid, 3-hydroxypropionic acid, and lactic acid into the degradable copolyester, the degradation is faster in the marine environment, buffer environment, and enzyme solution, and the degradation rate can be adjusted according to the content of the hydroxy fatty acid structural unit. At the same time, compared with the commercialized PBAT structure, the introduction of hydroxy fatty acids or their esterified structural monomers does not destroy its elastic modulus, tensile strength, and melting temperature, but has significantly improved the gas barrier performance.
[0145] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0146] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a degradable copolyester, It is characterized in that The steps include: Under a protective atmosphere, a first monomer, a second monomer, and a third monomer are mixed with an esterification catalyst for esterification reaction to obtain a polyester oligomer, wherein the first monomer is selected from terephthalic acid or an ester thereof, the second monomer is selected from an aliphatic dibasic acid or an ester thereof, and the third monomer is selected from ethylene glycol or 1,4-butanediol, wherein the ratio of the sum of the molar amounts of the first monomer and the second monomer to the molar amount of the third monomer is 1:1.2-1:2.0; Under a protective atmosphere, mixing a fourth monomer with a condensation catalyst for condensation reaction to obtain a polyhydroxy fatty acid oligomer, wherein the fourth monomer is selected from a hydroxy fatty acid or an ester thereof; Under vacuum conditions, the polyester oligomer, the polyhydroxyalkanoic acid oligomer and a polycondensation catalyst are mixed to perform a melt polycondensation reaction to obtain a degradable copolyester, wherein the ratio of the sum of the molar amounts of the second monomer and the fourth monomer to the molar amount of the first monomer is 3:2-2:3, and the molar ratio of the second monomer to the fourth monomer is 9:1-1:9; The structural formula of the degradable copolyester is shown in the following formula (1): In formula (1), R 1 , R 3 The structural units are independently selected from ethylene glycol or 1,4-butanediol, R 2 A structural unit selected from an aliphatic dibasic acid or an ester thereof, R 4 A structural unit selected from hydroxy fatty acids or esters thereof, wherein x, y, z, and m are all integers, x=1-10, y=1-10, z=1-10, and m=20-100; Among them, R 2 and R 4 The sum of the molar amounts of The molar ratio of R 2 With R 4 The molar ratio is 9:1-1:
9.
2. The method for preparing the degradable copolyester according to claim 1, It is characterized in that The R 4 A structural unit selected from hydroxy fatty acids having 2 to 5 carbon atoms or esters thereof.
3. The method for preparing the degradable copolyester according to claim 2, It is characterized in that The hydroxy fatty acid or its ester is selected from at least one of glycolic acid, esters of glycolic acid, 3-hydroxypropionic acid, esters of 3-hydroxypropionic acid, 4-hydroxybutyric acid, esters of 4-hydroxybutyric acid, lactic acid, and esters of lactic acid.
4. The method for preparing the degradable copolyester according to claim 1, It is characterized in that The aliphatic dibasic acid or its ester is selected from at least one of malonic acid, esters of malonic acid, succinic acid, esters of succinic acid, glutaric acid, esters of glutaric acid, adipic acid, esters of adipic acid, suberic acid, esters of suberic acid, azelaic acid, esters of azelaic acid, sebacic acid, and esters of sebacic acid.
5. The method for preparing the degradable copolyester according to claim 1, It is characterized in that The intrinsic viscosity of the degradable copolyester is 0.8 dL / g-1.5 dL / g, and the number average molecular weight is 35000 g / mol-60000 g / mol.
6. The method for preparing the degradable copolyester according to claim 1, It is characterized in that In the step of mixing the polyester oligomer, the polyhydroxyalkanoic acid oligomer and the polycondensation catalyst to carry out melt polycondensation reaction, a stabilizer is also added.
7. The method for preparing the degradable copolyester according to claim 1, It is characterized in that The esterification reaction temperature is 140°C-155°C, and the time is 4h-7h; And / or, the condensation reaction temperature is 120°C-180°C, and the time is 5h-10h; And / or, the temperature of the melt polycondensation reaction is 180°C-210°C, the time is 5h-10h, and the melt polycondensation reaction is carried out under the condition of vacuum degree less than or equal to 30Pa.