A fine recycling method and recycling device for lithium / sodium ion battery pole piece scraps

By using a roll-to-roll dry recycling method, the organic binders of lithium-ion battery scraps are stripped off at high temperatures. Combined with ultrasonic sieving and plasma treatment, this method achieves efficient, low-cost, and waste-free fine recycling of lithium-ion battery scraps, making it suitable for large-scale production.

CN115498302BActive Publication Date: 2024-11-15HUAZHONG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211324612.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-27
Publication Date
2024-11-15
Estimated Expiration
2042-10-27

AI Technical Summary

Technical Problem

Existing methods for recycling scraps from lithium-ion batteries damage the structure of active materials, resulting in high energy consumption, high cost, and difficulty in scaling up. Furthermore, traditional methods generate waste liquid discharge and environmental pressure.

Method used

The roll-to-roll dry recycling method is adopted, which separates the active material from the current collector by peeling off the organic binder of the active layer at high temperature, and achieves fine recycling through steps such as ultrasonic sieving and plasma treatment, thus avoiding waste liquid discharge.

Benefits of technology

It achieves efficient separation and recycling of active materials, reduces energy consumption and environmental pollution, is suitable for large-scale production, and is compatible with existing battery production processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115498302B_ABST
    Figure CN115498302B_ABST
Patent Text Reader

Abstract

The present invention discloses a method and device for fine recycling of positive and negative electrode scraps of lithium / sodium ion batteries, the method comprising the following steps: (1) unwinding a waste roll of electrode scraps and passing it through a high-temperature heat source at a uniform speed, so that the organic binder in the active layer is carbonized and ineffective, and at the same time, the active material and the current collector metal foil are separated; (2) grinding the obtained active material block to obtain active material powder; (3) treating the obtained active material powder with an ultrasonic vibration screen to separate the carbon black conductive agent and the active material powder to obtain an active material; (4) performing surface decontamination, polishing and flattening treatment on the obtained current collector metal foil to obtain high-quality recycled metal foil. The present invention realizes the rapid separation and fine recycling of scraps without destroying the structure of the active material. The method of the present invention has the advantages of high efficiency, low cost and simple process, is suitable for large-scale mass production, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of energy materials, and in particular relates to a fine recycling method and a recycling device for lithium / sodium ion battery pole piece scraps. Background Art

[0002] With the proposal of the "dual carbon" goal in 2020, my country has significantly accelerated the transformation of its energy structure, and will gradually transition from traditional fossil energy to clean energy dominated by hydropower, wind power, solar energy, etc. It is estimated that by 2025, lithium-ion batteries will occupy 70% of the new energy market. As waste in the production process of positive and negative poles of lithium-ion batteries, the output of pole scraps will grow rapidly year-on-year with the output of lithium-ion batteries. However, since the scraps have not yet been assembled into batteries, the active substances still have excellent electrochemical properties, with an active material content of more than 80%. Therefore, the recycling and reuse of scraps has important positive significance for the global resource shortage and energy crisis.

[0003] At present, the recycling methods of waste lithium-ion batteries in the industry mainly include: pyrometallurgy and hydrometallurgy. Pyrometallurgy uses high-temperature smelting, and its main recycled products are metal alloys, and there are large amounts of carbon dioxide emissions. Hydrometallurgy uses high-concentration acid and alkali to dissolve the pole pieces, converting inorganic active substances into ions, and finally drying to obtain metal salt precursors. For waste lithium-ion battery pole pieces, since their active materials and even the current collector metal foils have a certain degree of structural damage, the above two methods have good applicability. The structure and function of the active materials in the lithium-ion battery scraps are intact. If the above two methods are used for treatment, the structure of the material will be completely destroyed. The reuse process still requires the obtained precursor to be re-synthesized into a usable positive electrode material or current collector metal foil, which artificially prolongs the recycling process, consumes more energy, increases the economic cost of recycling and increases environmental pressure.

[0004] Some studies have shown that direct recycling of positive and negative active materials in waste lithium-ion batteries can be achieved, such as electrolysis, liquid phase ultrasound, traditional low-temperature calcination, molten salt method, etc. However, the above methods have problems such as large amounts of waste liquid discharge, high energy consumption, difficulty in scalability, and incompatibility with existing lithium / sodium ion battery production processes. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the present invention provides a roll-to-roll fine recycling method and recycling device for the positive and negative electrode scraps of lithium / sodium ion batteries, the purpose of which is to achieve rapid separation and fine recycling of the scraps without destroying the structure of the active material. The method of the present invention has the advantages of high efficiency, low cost, simple process, convenient operation, no waste liquid discharge, no secondary pollution of battery materials, and high value of recycled materials. It is particularly suitable for large-scale mass production and has a good application prospect.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A fine recycling method for positive and negative electrode scraps of lithium / sodium ion batteries comprises the following steps:

[0008] (1) Feeding: The scraps are passed through the rollers and the waste electrodes are flattened by rolling.

[0009] (2) High-temperature stripping: The waste positive and negative electrode scraps after extrusion are passed through a high-temperature heat source at a uniform speed, causing the organic binder in the active layer to carbonize and become ineffective, thereby achieving the separation of the active material and the current collector;

[0010] (3) Material collection: The separated active materials are collected through a collecting funnel, and the complete current collector metal foil is finally collected by winding;

[0011] (4) crushing the active material block: grinding the active material block obtained in step (3) to obtain active material powder;

[0012] (5) Screening to remove the carbon black conductive agent: The active material powder obtained in step (4) is treated with an ultrasonic vibration screen to separate the small-sized carbon black conductive agent and the active material powder, thereby obtaining the active material.

[0013] (6) Decontamination of the current collector metal foil: Physically and chemically clean the surface of the metal foil obtained in step (3) to remove surface residues with the assistance of a cleaning agent;

[0014] (7) Polishing the current collector metal foil: Plasma treatment is performed on the metal foil obtained in step (6) to further remove trace impurities on the surface;

[0015] (8) Shaping of the current collector metal foil: The metal foil obtained in step (7) is passed through a roller shaft and hot-pressed and flattened under the protection of an inert atmosphere to obtain a regenerated metal foil.

[0016] As one of the preferred solutions, the electrode in step (1) is a positive electrode or a negative electrode of a lithium ion battery or a sodium ion battery.

[0017] As one of the preferred solutions, the temperature of the high temperature heat source in step (1) is 500-2000°C.

[0018] As one of the preferred solutions, the uniform speed in step (1) is 0.01 to 10 m / s.

[0019] As one of the preferred solutions, the distance between the waste roll and the high-temperature heat source in step (1) is 1 to 2 cm.

[0020] As one of the preferred solutions, the current collector metal foil in step (2) is copper foil or aluminum foil; the active material is one or more of graphite, silicon-carbon negative electrode material, lithium cobalt oxide, lithium iron phosphate, and lithium nickel manganese oxide.

[0021] As one of the preferred solutions, the mesh size of the ultrasonic vibration screen is 500 to 1500 meshes;

[0022] As one of the preferred solutions, the material for surface physical and chemical cleaning is cotton and linen cloth, acrylic cloth, spandex cloth, viscose cloth, acetate cloth, coral fleece cloth, composite cloth, melt-blown cloth, sponge, etc.;

[0023] As one of the preferred solutions, the cleaning agent includes washing powder, dishwashing liquid, baking soda solution, toothpaste, etc.;

[0024] As one of the preferred solutions, the gas for generating plasma includes: argon, hydrogen, oxygen, nitrogen, helium and a mixture of the above gases;

[0025] As one of the preferred embodiments, the inert atmosphere gas in step (8) includes nitrogen, argon, helium, or carbon dioxide;

[0026] As one of the preferred solutions, the temperature of hot pressing and flattening is 400 to 1200 degrees Celsius.

[0027] The present invention also claims protection for a recycling device for the dry recycling method of the above-mentioned lithium / sodium ion battery positive and negative electrode scraps, comprising a device body, wherein one side of the device body is provided with an unwinding roller, a first support roller, an upper heat source generator, a second support roller, an upper scraper, a third support roller, a lower heat source generator, a fourth support roller, a lower scraper, a winding power roller and a material receiving bin;

[0028] The unwinding roller is located at the upper right corner of one side of the device body, the upper scraper is located at the middle position of the left part of one side of the device body, and a first support roller and a second support roller are arranged between the unwinding roller and the upper scraper in sequence; an upper heat source generator is arranged between the first support roller and the second support roller;

[0029] The lower scraper is located at the lower right corner of one side of the device body, and a third support roller and a fourth support roller are arranged between the upper scraper and the lower scraper in sequence; a lower heat source generator is arranged between the third support roller and the fourth support roller;

[0030] The upper scraper blade faces left, and the lower scraper blade faces right;

[0031] The winding power roller is located in the middle of the bottom of one side of the device body and is connected to the motor rotating shaft in the device body;

[0032] The material receiving bin is located at the bottom of the winding power roller;

[0033] The upper heat source generator and the lower heat source generator are electric heaters.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] (1) The recovery method of the present invention is a dry method without waste liquid discharge; the recovery process is short, the operation is simple, the heat treatment time per unit area is short, and the energy consumption is low.

[0036] (2) The present invention uses rapid heating to carbonize the organic binder and render it ineffective, thereby achieving direct and efficient separation of the active material and the current collector metal foil, thereby avoiding contamination of the active material by the current collector metal element.

[0037] (3) The present invention realizes the recovery and regeneration of the complete metal foil while recovering the active material.

[0038] (4) The roll-to-roll processing method adopted by the present invention is compatible with the existing battery electrode production process and is very suitable for large-scale mass production. After the scraps are cut, they can be separated and recycled in situ online, which can reduce the space occupied by the scraps in the warehouse; the rolled scraps can also be unrolled and recycled. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 is a flow chart of the recovery method of the present invention;

[0040] Figure 2 It is a schematic diagram of a device and process for separating graphite active material and copper foil current collector in the recycling method of the present invention;

[0041] Figure 3 This is a product picture of the copper foil roll and graphite powder block obtained after separation in Example 1 of the present invention;

[0042] Figure 4 is a schematic diagram of the recovery device used in Example 1 of the present invention;

[0043] Figure 5 It is a front view of the recovery device used in Example 1 of the present invention. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0045] Example 1

[0046] A method for finely recycling negative electrode scraps of lithium-ion batteries comprises the following steps:

[0047] (1) The graphite negative electrode scraps are passed through the roller shaft, and the waste electrode pieces are flattened by rolling;

[0048] (2) Carbonization failure of binder: In the protective atmosphere of argon gas at normal pressure, the flattened graphite negative electrode scrap roll is unwound at a speed of 0.01 m / s and passed through a high-temperature heat source of 1000 degrees Celsius at a uniform speed, causing the organic binder in the active layer to carbonize and fail;

[0049] (3) Separating the active material block from the current collector metal foil: bending the copper foil electrode piece treated in step (2) to separate the graphite and the copper foil;

[0050] (4) crushing the active material block: grinding the powdered graphite obtained in step (3) to obtain graphite powder;

[0051] (5) Screening to remove the carbon black conductive agent: The graphite powder obtained in step (3) is treated with a 1000-mesh ultrasonic vibration screen to separate the small-sized carbon black conductive agent and the graphite powder, thereby obtaining graphite powder;

[0052] (6) Decontamination of the current collector copper foil: Physically and chemically clean the surface of the copper foil obtained in step (3) to remove surface residues with the assistance of a cleaning agent;

[0053] (7) Polishing the current collector copper foil: Plasma treatment is performed on the copper foil obtained in step (6) to further remove trace impurities on the surface;

[0054] (8) Shaping of the current collector copper foil: The copper foil obtained in step (7) is passed through a roller shaft and hot-pressed and flattened under the protection of an inert atmosphere to obtain a recycled metal foil.

[0055] Example 2

[0056] A roll-to-roll dry recycling method for lithium-ion battery negative electrode scraps comprises the following steps:

[0057] (1) The graphite negative electrode scraps are passed through the roller shaft, and the waste electrode pieces are flattened by rolling;

[0058] (2) Carbonization failure of binder: In the protective atmosphere of argon gas at normal pressure, the flattened graphite negative electrode scrap roll is unwound at a speed of 1 meter per second and passed through a high-temperature heat source of 2000 degrees Celsius at a uniform speed, causing the organic binder in the active layer to carbonize and fail;

[0059] (3) Separating the active material block from the current collector metal foil: bending the copper foil electrode piece treated in step (2) to separate the graphite and the copper foil;

[0060] (4) crushing the active material block: grinding the powdered graphite obtained in step (3) to obtain graphite powder;

[0061] (5) Screening to remove the carbon black conductive agent: The graphite powder obtained in step (3) is treated with a 1000-mesh ultrasonic vibration screen to separate the small-sized carbon black conductive agent and the graphite powder, thereby obtaining graphite powder;

[0062] (6) Decontamination of the current collector copper foil: Physically and chemically clean the surface of the copper foil obtained in step (3) to remove surface residues with the assistance of a cleaning agent;

[0063] (7) Polishing the current collector copper foil: Plasma treatment is performed on the copper foil obtained in step (6) to further remove trace impurities on the surface;

[0064] (8) Shaping of the current collector copper foil: The copper foil obtained in step (7) is passed through a roller shaft and hot-pressed and flattened under the protection of an inert atmosphere to obtain a recycled metal foil.

[0065] Example 3

[0066] A roll-to-roll dry recycling method for sodium ion battery negative electrode scraps comprises the following steps:

[0067] (1) The hard carbon negative electrode scraps are rolled through a pair of rollers, and the waste electrode pieces are flattened by rolling;

[0068] (2) Carbonization failure of binder: In the protective atmosphere of argon gas at normal pressure, the flattened hard carbon negative electrode scrap roll is unwound at a speed of 0.1 m / s and passed through a high-temperature heat source at 700 degrees Celsius at a uniform speed, causing the organic binder in the active layer to carbonize and fail;

[0069] (3) Separating the active material block from the current collector metal foil: bending the aluminum foil electrode piece treated in step (2) to separate the hard carbon from the aluminum foil;

[0070] (4) crushing the active material block: grinding the powder block hard carbon obtained in step (3) to obtain hard carbon powder;

[0071] (5) Screening to remove the carbon black conductive agent: The hard carbon powder obtained in step (3) is treated with a 1000-mesh ultrasonic vibration screen to separate the small-sized carbon black conductive agent and the hard carbon powder, thereby obtaining the hard carbon powder;

[0072] (6) Decontamination of the current collector aluminum foil: Physically and chemically clean the surface of the aluminum foil obtained in step (3) to remove surface residues with the assistance of a cleaning agent;

[0073] (7) Polishing the current collector aluminum foil: Plasma treatment is performed on the aluminum foil obtained in step (6) to further remove trace impurities on the surface;

[0074] (8) Shaping of the current collector aluminum foil: The aluminum foil obtained in step (7) is passed through a roller shaft and hot-pressed and flattened under the protection of an inert atmosphere to obtain a recycled metal foil.

[0075] Example 4

[0076] A roll-to-roll dry recycling method for lithium-ion battery positive electrode scraps comprises the following steps:

[0077] (1) passing the lithium iron phosphate positive electrode scraps through the roller shaft, and flattening the waste electrode pieces by rolling;

[0078] (2) Carbonization failure of binder: In the protective atmosphere of argon gas at normal pressure, the flattened lithium iron phosphate positive electrode scrap roll is unwound at a speed of 0.01 meters per second and passed through a high-temperature heat source at 500 degrees Celsius at a uniform speed, causing the organic binder in the active layer to carbonize and fail;

[0079] (3) Separating the active material block from the current collector metal foil: bending the aluminum foil electrode piece treated in step (2) to separate the lithium iron phosphate and the aluminum foil;

[0080] (4) crushing the active material block: grinding the powdery block of lithium iron phosphate obtained in step (3) to obtain lithium iron phosphate powder;

[0081] (5) Screening to remove the carbon black conductive agent: The lithium iron phosphate powder obtained in step (3) is treated with a 2000-mesh ultrasonic vibration screen to separate the small-sized carbon black conductive agent and the lithium iron phosphate powder, thereby obtaining the lithium iron phosphate powder;

[0082] (6) Decontamination of the current collector aluminum foil: Physically and chemically clean the surface of the aluminum foil obtained in step (3) to remove surface residues with the assistance of a cleaning agent;

[0083] (7) Polishing the current collector aluminum foil: Plasma treatment is performed on the aluminum foil obtained in step (6) to further remove trace impurities on the surface;

[0084] (8) Shaping of the current collector aluminum foil: The aluminum foil obtained in step (7) is passed through a roller shaft and hot-pressed and flattened under the protection of an inert atmosphere to obtain a recycled metal foil.

[0085] Example 5

[0086] A roll-to-roll dry recycling method for lithium-ion battery positive electrode scraps comprises the following steps:

[0087] (1) passing the leftover nickel-cobalt-manganese-oxide lithium positive electrode material through a roller shaft, and flattening the waste electrode piece by rolling;

[0088] (2) Carbonization failure of binder: In the protective atmosphere of argon gas at normal pressure, the flattened nickel cobalt manganese oxide lithium positive electrode scrap roll is unwound at a speed of 0.01 meters per second and passed through a high-temperature heat source of 500 degrees Celsius at a uniform speed, causing the organic binder in the active layer to carbonize and fail;

[0089] (3) Separating the active material block from the current collector metal foil: bending the aluminum foil electrode piece treated in step (2) to separate the lithium nickel cobalt manganese oxide from the aluminum foil;

[0090] (4) crushing the active material block: grinding the powder block of lithium nickel cobalt manganese oxide obtained in step (3) to obtain lithium nickel cobalt manganese oxide powder;

[0091] (5) Screening to remove the carbon black conductive agent: The nickel cobalt manganese oxide powder obtained in step (3) is treated with a 2000-mesh ultrasonic vibration screen to separate the small-sized carbon black conductive agent and the nickel cobalt manganese oxide powder, thereby obtaining the nickel cobalt manganese oxide powder;

[0092] (6) Decontamination of the current collector aluminum foil: Physically and chemically clean the surface of the aluminum foil obtained in step (3) to remove surface residues with the assistance of a cleaning agent;

[0093] (7) Polishing the current collector aluminum foil: Plasma treatment is performed on the aluminum foil obtained in step (6) to further remove trace impurities on the surface;

[0094] (8) Shaping of the current collector aluminum foil: The aluminum foil obtained in step (7) is passed through a roller shaft and hot-pressed and flattened under the protection of an inert atmosphere to obtain a recycled metal foil.

[0095] Example 6

[0096] like Figure 4-5 As shown, a dry recovery device for positive and negative electrode scraps of lithium / sodium ion batteries includes a device body 100, and one side of the device body 100 is provided with a rewinding roller 200, a first support roller 310, an upper heat source generator 410, a second support roller 320, an upper scraper 510, a third support roller 330, a lower heat source generator 420, a fourth support roller 340, a lower scraper 520, a winding power roller 600 and a material receiving bin 700.

[0097] In this embodiment, the unwinding roller 200 is located at the upper right corner of one side of the device body 100, the upper scraper 510 is located at the middle position of the left part of one side of the device body 100, and the first support roller 310 and the second support roller 320 are arranged between the unwinding roller 200 and the upper scraper 510 in sequence; an upper heat source generator 410 is arranged between the first support roller 310 and the second support roller 320.

[0098] In this embodiment, the lower scraper 520 is located at the lower right corner of one side of the device body 100, and the third support roller 330 and the fourth support roller 340 are respectively arranged between the upper scraper 510 and the lower scraper 520; a lower heat source generator 420 is arranged between the third support roller 330 and the fourth support roller 340.

[0099] In this embodiment, the blade of the upper scraper 510 faces left, and the blade of the lower scraper 520 faces right.

[0100] In this embodiment, the winding power roller 600 is located in the middle of the bottom of one side of the device body 100 and is connected to the motor rotation shaft in the device body 100; the rotation speed of the winding power roller is controlled by the motor.

[0101] In this embodiment, the material receiving bin 700 is located at the bottom of the winding power roller 600 .

[0102] In this embodiment, the upper heat source generator 410 and the lower heat source generator 420 are electric heaters.

[0103] In this embodiment, under the protective atmosphere of normal pressure argon gas, the motor drives the winding power roller 600 to rewind at a speed of 0.01 meters per second, and drives the unwinding roller 200 to unwind at a speed of 0.01 meters per second through the action on the scrap roll; supported by the first support roller 310 and the second support roller 320, the scrap roll passes under the upper heat source generator 320 at 1000 degrees Celsius at a speed of 0.01 meters per second, so that the organic binder in the active layer on one side of the scrap roll is carbonized and ineffective; then the upper scraper 510 bends the processed scrap roll , so that the graphite and copper foil on one side of the scrap roll are separated; then, supported by the third support roller 330 and the fourth support roller 340, the scrap roll passes under the lower heat source generator 340 at 1000 degrees Celsius at a speed of 0.01 meters per second, so that the organic binder in the active layer on the other side of the scrap roll is carbonized and ineffective; then the lower scraper 520 bends the treated copper foil electrode to separate the graphite and copper foil on the other side of the scrap roll; the completely separated graphite falls into the collecting bin 700 for recovery, and the separated copper foil is rolled into a roll by the winding power roller 600 for recovery.

[0104] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A dry recovery device for positive and negative electrode scraps of lithium / sodium ion batteries, characterized in that: The device comprises a device body (100), wherein one side of the device body (100) is provided with an unwinding roller (200), a first supporting roller (310), an upper heat source generator (410), a second supporting roller (320), an upper scraper (510), a third supporting roller (330), a lower heat source generator (420), a fourth supporting roller (340), a lower scraper (520), a winding power roller (600) and a material receiving bin (700); The unwinding roller (200) is located at the upper right corner of one side of the device body (100); the upper scraper (510) is located at the middle position of the left part of one side of the device body (100); a first support roller (310) and a second support roller (320) are provided in sequence between the unwinding roller (200) and the upper scraper (510); an upper heat source generator (410) is provided between the first support roller (310) and the second support roller (320); The lower scraper (520) is located at the lower right corner of one side of the device body (100); a third support roller (330) and a fourth support roller (340) are provided in sequence between the upper scraper (510) and the lower scraper (520); a lower heat source generator (420) is provided between the third support roller (330) and the fourth support roller (340); The blade of the upper scraper (510) faces leftward, and the blade of the lower scraper (520) faces rightward; The winding power roller (600) is located in the middle of the bottom of one side of the device body (100) and is connected to the motor rotation shaft in the device body (100); The material receiving bin (700) is located at the bottom of the winding power roller (600); The upper heat source generator (410) and the lower heat source generator (420) are electric heaters; The scrap roll is supported by the first support roller (310) and the second support roller (320) and passes under the upper heat source generator (410). The scrap roll is supported by the third support roller (330) and the fourth support roller (340) and passes under the lower heat source generator (420).

2. A recycling method using the dry recycling device for positive and negative electrode scraps of lithium / sodium ion batteries according to claim 1, characterized in that: The steps include: (1) Carbonization failure of binder: Under the protection of normal pressure and inert atmosphere, the pole piece scrap waste roll is unwound and passed through a high-temperature heat source at a uniform speed, causing the organic binder in the active layer to carbonize and fail; (2) Separation of the active material block from the current collector metal foil: Apply a certain tensile tension to the current collector metal foil electrode after the treatment in step (1) to separate the active material from the current collector metal foil.

3. The recycling method according to claim 2, characterized in that: The steps also include: (3) crushing the active material block: grinding the active material block obtained in step (2) to obtain active material powder; (4) Screening to remove the carbon black conductive agent: The active material powder obtained in step (3) is treated with an ultrasonic vibration screen to separate the small-sized carbon black conductive agent and the active material powder, thereby obtaining the active material.

4. The recycling method according to claim 2, characterized in that: The inert atmosphere in step (1) is argon or nitrogen.

5. The recycling method according to claim 2, characterized in that: The electrode sheet in step (1) is a positive electrode sheet or a negative electrode sheet of a lithium ion battery or a sodium ion battery.

6. The recycling method according to claim 2, characterized in that: The temperature of the high temperature heat source in step (1) is 500-2000°C.

7. The recycling method according to claim 2, characterized in that: The uniform speed in step (1) is 0.01-10 m / s.

8. The recycling method according to claim 2, characterized in that: The distance between the waste roll and the high-temperature heat source in step (1) is 1 to 2 cm.

9. The recycling method according to claim 2, characterized in that: The method of applying tension in step (2) is to bend the pole piece more than 90 degrees so that the pole piece is taut and slides over a smooth edge.

10. The recycling method according to claim 2, characterized in that: The current collector metal foil in step (2) is copper foil or aluminum foil, and the active material is one or more of graphite, silicon-carbon negative electrode material, lithium cobalt oxide, lithium iron phosphate, and lithium nickel manganese oxide.