An instant heating wire-wound thick film heating element

By using instant-heat wire-wound thick film heating body in water appliances, the insulating medium and protective layer formed by cobalt blue and iron red glazes is solved, and the existing heating body is slow to rise, high safety risks and high cost. The problem is to achieve rapid heating, safe and reliable and high temperature resistance.

CN115515265BActive Publication Date: 2024-12-06余定益
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211298430.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-23
Publication Date
2024-12-06
Estimated Expiration
2042-10-23

AI Technical Summary

Technical Problem

In the existing water appliance heating technology, the heating body has problems such as slow heating, low thermal efficiency, high safety risks, complex structure, high cost and poor durability, especially ordinary metal heating bodies, quartz tube nano-coated heating tubes and silicon nitride heating. The bodies have their own disadvantages, and the printed circuit thick film heating body is costly and easily damaged at high temperatures.

Method used

A ready-to-heat wire-wound thick film heating element is adopted, including a substrate, an insulating dielectric layer and a covering protective layer. The insulating dielectric layer is made of cobalt blue glaze and iron red glaze. The electric heating wire is wrapped around the insulating dielectric layer. It is also wrapped in a protective layer, and a high-temperature melting and sintering process is used to form a structure that is highly resistant to high temperature and has good thermal conductivity.

Benefits of technology

It achieves rapid heating, safety and reliability, high temperature resistance, waterproofness and acid-base corrosion resistance, reduces costs, and is not easy to damage when used for a long time at high temperatures, and has perfect hydroelectric separation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115515265B_ABST
    Figure CN115515265B_ABST
Patent Text Reader

Abstract

The present invention discloses an instant heating wire-wound thick film heating element, which comprises a substrate, an insulating dielectric layer, an electric heating wire, and a covering protective layer in sequence; the insulating dielectric layer is coated on the substrate, the electric heating wire is wound on the substrate coated with the insulating dielectric layer, and the covering protective layer is coated on the electric heating wire. The instant heating wire-wound thick film heating element of the present invention has excellent properties such as high temperature resistance, super thermal conductivity, high insulation, good water resistance, good acid and alkali corrosion resistance, and comprehensive protection. The heating speed is very fast and has perfect water-electricity separation. Through the production process of the present invention, various problems that have long existed in previous heating elements are fundamentally solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water household electrical heating, and in particular to an instant heating type wire-wound thick film heating element. Background Art

[0002] With the progress and development of society, people's living standards are becoming increasingly rich, and the demand for various household appliances is also increasing. Water appliances (such as water dispensers, tea bar machines, water heaters, pipeline machines, electric faucets, small kitchen treasures, etc.) are an indispensable part of people's daily life, bringing a qualitative improvement to people's lives.

[0003] Now, with the improvement of people's living standards, the acceleration of the pace, and the enhancement of safety awareness, people pay more and more attention to the quality and safety performance of products (especially water appliances). In the development of water appliance heating technology in the past few decades, various manufacturers have used many different production heating methods, heating materials and production processes, hoping to maximize the competitiveness of their products. For example: ordinary metal heating elements, quartz tube nano-coated heating tubes, silicon nitride heating elements, printed circuit thick film heating elements, etc. But they all have different disadvantages. The disadvantages of ordinary metal heating elements are 1) slow heating and low thermal efficiency; 2) high-power heating elements are directly placed in water for heating. There is no separation of water and electricity at all. Direct power is turned on for heating, which has a great risk of electric shock; 3) a large amount of scale is easily generated on the surface. After a long time of use, it is easy to cause water blockage and serious burning of the heating element. The disadvantages of quartz tube nano-coated heating tubes are: 1) the power is much smaller than that of other types of heating tubes under the same heating area. If it is to be made into high power, the structure will be very complicated and the volume will be large; 2) the power is unstable, the power will continue to decrease with the increase of temperature, and the power will be significantly attenuated after a certain period of use, and it cannot be restored; 3) the input end is a printed conductive silver paste ring, and then a metal ring is clamped on it. Because the quartz tube is too smooth, the printed conductive silver paste ring is very easy to fall off, and the metal ring is not tightly clamped. When the power is turned on, it is easy to spark at the poor contact point, which is very unsafe; 4) the quartz tube is a glass product, which is very easy to break and is not easy to transport and install as a single tube. The disadvantages of silicon nitride heating elements are: 1) the price is very expensive; 2) the structural design is very complicated, it cannot be used directly, and it must be made of aluminum with good thermal conductivity as the base material, and the shell is made by die-casting first, and then fine-processed and installed on the silicon nitride heating element; 3) the overall volume is also large and the weight is also heavy; 4) it cannot be used at high temperatures exceeding 400 degrees because the aluminum shell cannot withstand it. Printed circuit thick film heating elements have always had the best heating performance in the heating field. They have the advantages of fast heating, high thermal efficiency, and water-electricity separation. However, they cannot be popularized because the use of precious metals in their slurries makes their costs high, and the production process requirements are also very stringent. Moreover, in high-temperature dry-burning experiments, as long as the temperature is raised to above 400 degrees, there is a risk of burning the printed resistance heating circuit. If the temperature is raised to above 600 degrees, the resistance heating circuit will be burned, causing direct damage to the heating element.

[0004] Because all kinds of heating elements on the market have various shortcomings, there is an urgent need for an instant wire-wound thick-film heating element with excellent overall performance and low cost to be studied. Summary of the invention

[0005] In view of the problems in the prior art, the present invention provides an instant heating wire-wound thick film heating element with excellent performance, safety, reliability and low cost. The specific technical solution is as follows:

[0006] An instant heating wire-wound thick film heating element comprises a substrate, an insulating medium layer, a heating wire, and a covering protective layer in sequence;

[0007] The insulating medium layer is coated on a substrate, the heating wire is wound on the substrate coated with the insulating medium layer, and the covering protective layer is coated on the heating wire.

[0008] Preferably, the insulating medium is a cobalt blue glaze. Calculated by weight, the raw materials of the cobalt blue glaze include 9 to 13 parts of anhydrous borax, 12 to 20 parts of sodium carbonate, 4 to 7 parts of calcite, 22 to 31 parts of potassium feldspar, 5 to 10 parts of kaolin, 20 to 40 parts of quartz, 0.1 to 0.9 parts of titanium dioxide, 3 to 9 parts of zirconium silicate, 2 to 3 parts of strontium carbonate, 2 to 6 parts of barium carbonate, 1.5 to 3 parts of cobalt oxide, 0.8 to 2.2 parts of nickel oxide, 1 to 2 parts of zinc oxide, 0.5 to 2 parts of iron oxide, and 0.1 to 1 part of manganese dioxide.

[0009] Preferably, the method for preparing the insulating dielectric layer comprises the following steps:

[0010] (1) mixing the raw materials in a uniform ratio to form a cobalt blue glaze raw material;

[0011] (2) adding the uniformly mixed cobalt blue glaze raw materials into a high-temperature melting furnace at 1400-1500° C., melting the powdered raw materials into liquid, and then flowing the liquid into a cold water tank, and then being quenched by water to form cobalt blue glass-like particles, and then fishing out the particles to obtain a cobalt blue frit;

[0012] (3) drying the obtained cobalt blue frit, and grinding it into a fine powder that can pass through 320-330 meshes to obtain a cobalt blue glaze powder;

[0013] (4) Grinding the cobalt blue glaze powder and the ink oil in a ratio of 1:0.65-0.7 through a grinder to obtain a cobalt blue paste;

[0014] (5) After the cobalt blue paste is slurried, it is coated on the substrate, dried, and then sintered at high temperature to obtain an insulating dielectric layer.

[0015] Preferably, the covering protective layer is an iron red glaze, and the raw materials of the iron red glaze include, by weight, 10 to 16 parts of anhydrous borax, 8 to 12 parts of sodium carbonate, 4 to 7 parts of dolomite, 18 to 26 parts of potassium feldspar, 4 to 8 parts of kaolin, 20 to 30 parts of quartz, 10 to 16 parts of titanium dioxide, 2 to 3 parts of strontium carbonate, 2 to 4 parts of barium carbonate, 0.1 to 1 part of cobalt oxide, 1 to 2 parts of nickel oxide, 1 to 2 parts of zinc oxide, and 10 to 19 parts of iron oxide.

[0016] Preferably, the method for preparing the covering protective layer comprises the following steps:

[0017] (1) mixing the raw materials in accordance with a proportion to form an iron red glaze raw material;

[0018] (2) adding the uniformly mixed iron red glaze raw materials into a high-temperature melting furnace at 1400-1500° C., melting the powdered raw materials into liquid, and then flowing the liquid into a cold water tank, and then being quenched by water to become iron red glass-like particles, and then fishing out the particles to obtain an iron red frit;

[0019] (3) drying the obtained iron red frit, and grinding it into a fine powder that can pass through 320-330 meshes to obtain iron red glaze powder;

[0020] (4) grinding iron red glaze powder and ink oil in a ratio of 1:0.65-0.7 through a grinder to obtain iron red ointment;

[0021] (5) After the iron red ointment is slurried, it is coated on the electric heating wire, the electric heating wire is wrapped inside, and after drying, it is sintered at high temperature to obtain a covering protective layer.

[0022] Preferably, the substrate layer is made of SUS430 ferritic stainless steel.

[0023] Preferably, the heating wire is an iron-chromium-aluminum heating wire.

[0024] Preferably, the heating wire is wound around the substrate coated with the insulating medium layer and fixed by a clamp.

[0025] It can be seen from the above description that the present invention has the following advantages:

[0026] 1. The product of the present invention, the instant hot wire-wound thick film heating element, has excellent properties such as high temperature resistance, super thermal conductivity, high insulation, good waterproofness, good acid and alkali corrosion resistance, and comprehensive protection. Through the production process of the present invention, various long-standing problems of heating elements in the past are fundamentally solved.

[0027] 2. The product of the present invention has a very fast heating speed. Taking a heating tube with a diameter of 22mm, a length of 130mm and a power of 2200W as an example, at an ambient temperature of 25 degrees, the water temperature can immediately rise to more than 100 degrees within 2-3 seconds. At the same time, it has perfect water-electricity separation, which is safe and reliable.

[0028] 3. The product of the present invention has excellent high temperature resistance and anti-dry burning performance. It can be used for a long time at a high temperature of 1000 degrees and can withstand a high temperature of up to 1400 degrees for more than 10 seconds. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a cross-sectional schematic diagram of the product of the present invention.

[0030] In the figure: 1: substrate, 2: insulating medium layer, 3: heating wire, 4: covering protective layer. DETAILED DESCRIPTION

[0031] In order to explain the technical features of the present invention in detail, the features of the present invention are further described below through examples, but no limitation is imposed on the claims of the present invention.

[0032] like Figure 1 As shown, a preferred embodiment of the present invention provides an instant heating wire-wound thick film heating element, which comprises a substrate 1, an insulating medium layer 2, a heating wire 3, and a covering protective layer 4 in sequence;

[0033] The insulating medium layer 2 is coated on the substrate 1 , the heating wire 3 is wound on the substrate 1 coated with the insulating medium layer 2 , and the covering protective layer 4 is coated on the heating wire 3 .

[0034] The method for preparing the insulating dielectric layer 2 comprises the following steps:

[0035] (1) Mix the following raw materials in a uniform ratio to form a cobalt blue glaze raw material;

[0036] The raw material ratio is: 11.5 parts of anhydrous borax, 16 parts of sodium carbonate, 5.5 parts of calcite, 27 parts of potassium feldspar, 8 parts of kaolin, 30 parts of quartz, 0.5 parts of titanium dioxide, 6 parts of zirconium silicate, 2.6 parts of strontium carbonate, 4 parts of barium carbonate, 2.3 parts of cobalt oxide, 1.5 parts of nickel oxide, 1.5 parts of zinc oxide, 1 part of iron oxide, and 0.5 parts of manganese dioxide;

[0037] The requirements for raw materials are as follows:

[0038]

[0039]

[0040] The fineness of the above raw materials is required to be above 80 mesh.

[0041] (2) adding the uniformly mixed cobalt blue glaze raw materials into a high-temperature melting furnace at 1400-1500° C., melting the powdered raw materials into liquid, and then flowing the liquid into a cold water tank, and then being quenched by water to form cobalt blue glass-like particles, and then fishing out the particles to obtain a cobalt blue frit;

[0042] (3) drying the obtained cobalt blue frit, and grinding it into a fine powder that can pass through 320-330 meshes to obtain a cobalt blue glaze powder;

[0043] (4) Grinding the cobalt blue glaze powder and the ink oil in a ratio of 1:0.65-0.7 through a grinder to obtain a cobalt blue paste;

[0044] (5) After the cobalt blue paste is slurried, it is coated on the substrate, dried, and then sintered at a high temperature to obtain the insulating dielectric layer 2.

[0045] The preparation method of the covering protective layer 4 comprises the following steps:

[0046] (1) Mix the following raw materials in a uniform ratio to form iron red glaze raw material;

[0047] The raw material ratio is: 13 parts of anhydrous borax, 10 parts of sodium carbonate, 5.5 parts of dolomite, 22 parts of potassium feldspar, 6 parts of kaolin, 25 parts of quartz, 13 parts of titanium dioxide, 2.6 parts of strontium carbonate, 3 parts of barium carbonate, 0.5 parts of cobalt oxide, 1.5 parts of nickel oxide, 1.5 parts of zinc oxide, and 14 parts of iron oxide;

[0048] The requirements for raw materials are as follows:

[0049]

[0050]

[0051] The fineness of the above raw materials is required to be above 80 mesh

[0052] (2) adding the uniformly mixed iron red glaze raw materials into a high-temperature melting furnace at 1400-1500° C., melting the powdered raw materials into liquid, and then flowing the liquid into a cold water tank, and then being quenched by water to become iron red glass-like particles, and then fishing out the particles to obtain an iron red frit;

[0053] (3) drying the obtained iron red frit, and grinding it into a fine powder that can pass through 320-330 meshes to obtain iron red glaze powder;

[0054] (4) grinding iron red glaze powder and ink oil in a ratio of 1:0.65-0.7 through a grinder to obtain iron red ointment;

[0055] (5) After the iron red ointment is slurried, it is coated on the electric heating wire, the electric heating wire is wrapped inside, dried, and then sintered at high temperature to obtain a covering protective layer

[0056] This implementation obtains the parameters of the instant wire-wound thick film heating element:

[0057] Voltage: AC220V; Frequency: 50 / 60Hz; Power: 2200W;

[0058] Inner hole: 19mm; outer diameter: 22mm; length: 130mm; heating zone length: 93mm;

[0059] The thickness of the insulating dielectric layer is 0.3mm; the thickness of the covering protective layer is 0.5mm.

[0060] 1. High temperature resistance test

[0061] (1) Test method

[0062] Place the heating element upright on the workbench, connect a KSD301 jump-type thermostat, the temperature measuring point is 1.5mm away from the surface of the heating area, and connect AC220V voltage for testing.

[0063] (2) Test results

[0064]

[0065]

[0066] 2. Waterproof test

[0067] (1) Test method

[0068] Put the heating element as a whole into water, leave it there for a certain period of time, take it out and directly conduct a power-on test, and visually observe any adverse reactions of the heating element during the power-on process.

[0069] (2) Test results

[0070] Serial number Soaking time (h) Power-on test conditions (500°C) state 1 5 Power on and heat up to 500℃ No response 2 10 Power on and heat up to 500℃ No response 3 15 Power on and heat up to 500℃ No response 4 20 Power on and heat up to 500℃ No response 5 48 Power on and heat up to 500℃ No response 6 72 Power on and heat up to 500℃ No response 7 120 Power on and heat up to 500℃ No response

[0071] Note: The surface of the heating element tested above is covered with a protective layer with a thickness of 0.5 mm. The thicker the coating, the better the waterproofness.

[0072] 3. Acid and alkali resistance test

[0073] (1) Test method

[0074] The heating element is placed in alkaline liquid and acidic liquid in a certain proportion respectively. After being placed for a certain period of time, it is taken out and directly subjected to a power-on test to visually inspect any adverse reaction of the heating element during the power-on process.

[0075] (2) Test results

[0076]

[0077] 4. Insulation performance test

[0078] (1) Test method

[0079] Fix the heating element upright on a workbench, connect it to a high-voltage tester, and slowly increase the voltage of the high-voltage tester from small to large to conduct a test to observe the high-voltage bearing capacity of the heating element.

[0080] High voltage tester parameters:

[0081] Model: Meiruike RK2674A; Output voltage: AC / DC, 0~20KV;

[0082] Test current: AC, 0~20mA; DC, 0~10mA

[0083] Transformer capacity: 400VA

[0084] (2) Test results

[0085]

[0086]

[0087] According to the above test results, the instant heating wire-wound thick film heating element of the present invention has the following advantages:

[0088] 1. The product of the present invention, the instant hot wire-wound thick film heating element, has excellent properties such as high temperature resistance, super thermal conductivity, high insulation, good waterproofness, good acid and alkali corrosion resistance, and comprehensive protection. Through the production process of the present invention, various long-standing problems of heating elements in the past are fundamentally solved.

[0089] 2. The product of the present invention has a very fast heating speed and has perfect water-electricity separation, which is safe and reliable.

[0090] 3. The product of the present invention has excellent high temperature resistance and anti-dry burning performance. It can be used for a long time at a high temperature of 1000 degrees and can withstand a high temperature of up to 1400 degrees for more than 10 seconds.

[0091] It is understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.

Claims

1. An instant heating wire-wound thick film heating element, characterized in that: It includes a base material, an insulating medium layer, a heating wire, and a covering protective layer in sequence; The insulating medium layer is coated on the substrate, the heating wire is wound on the substrate coated with the insulating medium layer, and the covering protective layer is coated on the heating wire; The insulating medium is a cobalt blue glaze, and the raw materials of the cobalt blue glaze include, by weight, 9-13 parts of anhydrous borax, 12-20 parts of sodium carbonate, 4-7 parts of calcite, 22-31 parts of potassium feldspar, 5-10 parts of kaolin, 20-40 parts of quartz, 0.1-0.9 parts of titanium dioxide, 3-9 parts of zirconium silicate, 2-3 parts of strontium carbonate, 2-6 parts of barium carbonate, 1.5-3 parts of cobalt oxide, 0.8-2.2 parts of nickel oxide, 1-2 parts of zinc oxide, 0.5-2 parts of iron oxide, and 0.1-1 part of manganese dioxide; The covering protective layer is an iron red glaze. Calculated by weight, the raw materials of the iron red glaze include 10 to 16 parts of anhydrous borax, 8 to 12 parts of sodium carbonate, 4 to 7 parts of dolomite, 18 to 26 parts of potassium feldspar, 4 to 8 parts of kaolin, 20 to 30 parts of quartz, 10 to 16 parts of titanium dioxide, 2 to 3 parts of strontium carbonate, 2 to 4 parts of barium carbonate, 0.1 to 1 part of cobalt oxide, 1 to 2 parts of nickel oxide, 1 to 2 parts of zinc oxide, and 10 to 19 parts of iron oxide.

2. The instant heating wire-wound thick film heating element according to claim 1, characterized in that: The method for preparing the insulating dielectric layer comprises the following steps: (1) mixing the raw materials uniformly according to the proportion to form a cobalt blue glaze raw material; (2) Add the mixed cobalt blue glaze raw materials into a high-temperature melting furnace at 1400-1500℃, melt the powdered raw materials into liquid, and then flow into a cold water tank. After water quenching, the liquid becomes cobalt blue glass-like particles, and the particles are fished out to obtain cobalt blue frit; (3) drying the obtained cobalt blue frit and grinding it into a fine powder that can pass through 320-330 mesh to obtain cobalt blue glaze powder; (4) Grind the cobalt blue glaze powder and ink oil in a ratio of 1:0.65-0.7 in a grinder to obtain a cobalt blue paste; (5) After the cobalt blue paste is slurried, it is coated on the substrate, dried, and then sintered at high temperature to obtain an insulating dielectric layer.

3. The instant heating wire-wound thick film heating element according to claim 1, characterized in that: The method for preparing the covering protective layer comprises the following steps: (1) mixing the raw materials uniformly according to the proportion to form iron red glaze raw material; (2) Add the mixed iron red glaze raw materials into a high-temperature melting furnace at 1400-1500℃, melt the powdered raw materials into liquid, and then flow into a cold water tank. After water quenching, the liquid becomes iron red glass-like particles, and the particles are fished out to obtain iron red frit; (3) drying the obtained iron red frit, and grinding it into a fine powder that can pass through 320-330 mesh to obtain iron red glaze powder; (4) Grind the iron red glaze powder and ink oil in a ratio of 1:0.65-0.7 in a grinder to obtain iron red ointment; (5) After the iron red paste is slurried, it is coated on the heating wire, the heating wire is wrapped inside, and after drying, it is sintered at high temperature to obtain a covering protective layer.

4. The instant heating wire-wound thick film heating element according to claim 1, characterized in that: The substrate layer is made of SUS430 ferrite stainless steel.

5. The instant heating wire-wound thick film heating element according to claim 1, characterized in that: The heating wire is an iron-chromium-aluminum heating wire.

6. The instant heating wire-wound thick film heating element according to claim 1, characterized in that: The heating wire is wound on the base material coated with the insulating medium layer and fixed by a clamp.