Preparation method of MIL-88@CoMg water electrolysis hydrogen evolution catalyst based on nickel foam

By using a foam nickel-based MIL-88@CoMg catalyst in the process of electrolyzing water hydrogen production, combined with the high catalytic activity of iron-cobalt-magnesium materials and the porous MOF structure, the problem of poor catalyst stability is solved, and efficient hydrogen production and stability is achieved catalytic properties.

CN115522215BActive Publication Date: 2024-11-12HENAN TONGWEIDIAN STONE HYDROGEN ENERGY TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211229392.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-09
Publication Date
2024-11-12
Estimated Expiration
2042-10-09

AI Technical Summary

Technical Problem

The existing catalysts have poor stability and poor catalytic effect in the process of electrolyzing hydrogen production, especially facing challenges of different pH and alkalinity and temperatures, which hinder the development of hydrogen energy technology.

Method used

Using MIL-88@CoMg catalyst based on nickel foam as the substrate, a hydrogen evolution catalyst with high catalytic activity and stability was prepared by combining the high catalytic activity and MOF porous structure of iron-cobalt magnesium materials, using the synergy between cobalt ions and magnesium ions. Effects to enhance the bonding ability of the material to the substrate.

Benefits of technology

It significantly improves the efficiency of hydrogen analysis of electrolytic water and the stability of the catalyst, and can be reused multiple times, significantly improving the conductivity and catalytic performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115522215B_ABST
    Figure CN115522215B_ABST
Patent Text Reader

Abstract

The present invention discloses a MIL-88@CoMg electrolysis water hydrogen production catalytic material based on nickel foam, which selects three metal elements of iron, cobalt and magnesium as the main elements of the catalyst, combines the high activity of transition metal catalytic hydrogen evolution with the MOF porous structure, and utilizes the high porosity of the MOF material to increase the relative specific surface area of ​​the hydrogen evolution material, improve the conductivity of the material, and thus greatly increase the hydrogen evolution efficiency of electrolysis water. At the same time, the synergistic effect of cobalt ions and magnesium ions can accelerate the adsorption of the active sites of the catalyst and the nickel foam substrate material, so that the binding ability of the material and the substrate is greatly increased during the catalytic process, and the catalytic stability is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of hydrogen energy, and specifically relates to a method for preparing a MIL-88@CoMg water electrolysis hydrogen evolution catalyst based on nickel foam. By combining the high catalytic activity of iron-cobalt-magnesium catalytic materials and the advantages of MOF porous structure, a hydrogen evolution catalyst with high catalytic activity and good stability is prepared. Background Art

[0002] The extensive use of traditional fossil fuels has caused the dual problems of energy crisis and environmental degradation, thus triggering an urgent need for clean and sustainable alternative energy. The technical difficulties in the preparation of renewable energy are one of the key technologies that restrict the development of renewable energy. In the new energy system, hydrogen energy is an ideal secondary energy source. Compared with other energy sources, hydrogen has a high calorific value and its combustion product is water. It is the most environmentally friendly energy source. It can be stored in high-pressure tanks in the form of gas or liquid phase, and can also be stored in hydrogen storage materials in the form of solid phase. Another unique characteristic of hydrogen is the simplicity of chemical bonds. When it releases energy quickly, it breaks and forms relatively few bonds. It has a high reaction rate constant and faster electrode process kinetics, and can release its energy by electrochemical methods. Therefore, hydrogen is considered to be the most promising energy carrier to replace traditional fossil fuels. As a clean, pollution-free renewable energy source, hydrogen can effectively solve energy and environmental problems. The hydrogen production reaction by water electrolysis is considered to be the reverse reaction of hydrogen combustion. The combination of the two constitutes a zero-carbon emission energy cycle system. The main problem with the current materials for catalytic water electrolysis is the poor stability of the known materials. The catalysts do not show good catalytic effects when faced with different pH values, temperatures and current intensities. Therefore, the promotion of water electrolysis hydrogen production technology has been greatly hindered.

[0003] Metal-organic framework materials (MOFs) are a type of coordination polymer that has developed rapidly in the past two decades. They have a three-dimensional pore structure and have the advantages of high porosity, low density, large specific surface area, regular pores, adjustable pore size, and topological structure diversity and tailorability. Among them, MIL-88 is a metal organic framework compound with a MOF structure with iron as the main element, which is widely used in the fields of catalytic sensing. The present invention combines the porous structure of MOF materials and the high catalytic activity of iron-cobalt-magnesium materials to prepare a MIL-88@CoMg hydrogen evolution catalyst based on nickel foam that can stably electrolyze water. Summary of the invention

[0004] The present invention relates to a method for preparing a MIL-88@CoMg water electrolysis hydrogen evolution catalyst based on nickel foam, which has the characteristics of high catalytic activity and good stability of iron-nickel catalyst for hydrogen evolution, and also combines the structural advantages of MOF materials such as multiple pores, high porosity and large specific surface area. The present invention is achieved through the following technical solutions:

[0005] S1. Preparation of porous MOF skeleton: Weigh 10-15 parts of ferric nitrate nonahydrate and 3 parts of fumaric acid, dissolve them in 50 parts of distilled water, stir them with a magnetic stirrer at 30-70°C for 10-15 minutes, then put them in a muffle furnace, heat them at 120-150°C for 4-7 hours, cool them down and centrifuge them to generate MIL-88 nanoparticles;

[0006] S2. Introducing cobalt into the MOF framework: Dissolve 1 part of the centrifuged MIL-88 particles and 1-4 parts of cobalt nitrate hexahydrate in 50 parts of ethanol, and treat in an oil bath at 100°C for 1 h to obtain MIL-88@Co;

[0007] S3: The prepared MIL-88@Co nanoparticles were centrifuged at 4000r / min for 5min, then dried with anhydrous ethanol, and sintered in a tubular furnace under N2 atmosphere at a heating rate of 2℃ / min, 130℃ for 1h, and 350℃ for 2.5h to convert the cobalt element into cobalt tetroxide to obtain MIL-88@Co3O4;

[0008] S4, weigh 0.4-1 parts of magnesium sulfate and 0.5 parts of MIL-88@Co3O4, use a tubular furnace to reduce Co3O4 under hydrogen conditions and introduce magnesium ions to form MIL-88@CoMg, the reaction conditions are: 400℃, 2h;

[0009] S5: Use 3M hydrochloric acid and anhydrous ethanol to clean 0.8*1.0cm 2 The nickel foam base material is prepared by weighing 0.007-0.01 parts of MIL-88@CoMg nanomaterials, 0.015 parts of carbon powder, 0.05 parts of 0.1 mg / μL PTFE, and 5 parts of ethanol, and putting them into an ultrasonic cleaner for 30 minutes. After drying, the mixture is evenly applied to the treated nickel foam surface to obtain the MIL-88@CoMg hydrogen evolution catalyst based on nickel foam.

[0010] The solid material used in this technical solution is 1g per portion, and the liquid material is 1mL per portion.

[0011] Preferably: the S1 weighs 10 g of ferric nitrate nonahydrate, 3 g of fumaric acid, and 50 mL of distilled water;

[0012] Preferably: the cobalt nitrate hexahydrate weighed in S2 is 1 g and the ethanol is 50 mL;

[0013] Preferably: the magnesium sulfate weighed in S4 is 0.4 g;

[0014] Preferably, the S5 weighs 0.007 g of MIL-88@CoMg nanomaterial, 0.015 g of carbon powder, 0.05 mL of 0.1 mg / μL PTFE, and 5 mL of ethanol.

[0015] The invention is beneficial in that:

[0016] 1. The preparation process of the hydrogen evolution catalyst prepared by the present invention is relatively simple. Three transition metals, iron, cobalt and magnesium, are selected as the main elements of the catalyst. The high activity of the transition metals in catalyzing hydrogen evolution is combined with the MOF porous structure. The high porosity of the MOF material is utilized to increase the relative specific surface area of ​​the hydrogen evolution material and improve the conductivity of the material, thereby greatly increasing the hydrogen evolution efficiency of the electrolysis of water.

[0017] 2. At the same time, the synergistic effect of cobalt ions and magnesium ions can accelerate the adsorption of the active sites of the catalyst and the nickel foam base material, which greatly increases the bonding ability between the material and the base during the catalytic process and improves the catalytic stability.

[0018] 3. The catalyst prepared by the present invention has good stability and can be reused many times. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a microstructure scanning image (100 μm) of Example 1 of the present invention.

[0020] Figure 2 This is a microstructure scanning image (2 μm) of Example 2 of the present invention.

[0021] Figure 3 The linear voltammetric scanning curves of Examples 1-3 of the present invention are shown.

[0022] Figure 4 It is the Tafel slope curve of Examples 1-3 of the present invention.

[0023] Figure 5 This is a voltage-time curve diagram of Example 1 of the present invention.

[0024] Figure 6 This is the cyclic voltammetry scanning curve of Example 3 of the present invention.

[0025] Figure 7 This is the double-layer capacitance curve of Example 3 of the present invention. DETAILED DESCRIPTION

[0026] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.

[0027] Example 1

[0028] S1. Preparation of porous MOF skeleton: 10 g of ferric nitrate nonahydrate and 3 g of fumaric acid were weighed and dissolved in 50 mL of distilled water. The mixture was stirred with a magnetic stirrer at 30 °C for 10 min. The mixture was then placed in a muffle furnace for high temperature treatment. The heating conditions were as follows: heating at 150 °C for 4 h, cooling and centrifuging to generate MIL-88 nanoparticles.

[0029] S2. Introducing cobalt into the MOF framework: Dissolve 1 g of the centrifuged MIL-88 particles and 1 g of cobalt nitrate hexahydrate in 50 mL of ethanol and treat in an oil bath at 100 °C for 1 h to obtain MIL-88@Co.

[0030] S3: The prepared MIL-88@Co nanoparticles were centrifuged at 4000r / min for 5min, then dried with anhydrous ethanol, and sintered in a tubular furnace under N2 atmosphere at a heating rate of 2℃ / min, 130℃ for 1h, and 350℃ for 2.5h to convert the cobalt element into cobalt tetroxide to obtain MIL-88@Co3O4;

[0031] S4, weigh 0.4g of magnesium sulfate and 0.5g of MIL-88@Co3O4, use a tubular furnace to reduce Co3O4 under hydrogen conditions and introduce magnesium ions to form MIL-88@CoMg, the reaction conditions are: 400℃, 2h;

[0032] S5: Use 3M hydrochloric acid and anhydrous ethanol to clean 0.8*1.0cm 2 The nickel foam base material is prepared by weighing 0.007 g of MIL-88@CoMg nanomaterial, 0.015 g of carbon powder, 0.05 mL of 0.1 mg / μL PTFE, and 5 mL of ethanol, and putting them into an ultrasonic cleaner for 30 min. After drying, the mixture is evenly applied to the treated nickel foam surface to obtain the MIL-88@CoMg hydrogen evolution catalytic material with nickel foam as the base material.

[0033] Comparative Example 1: In step S1, except that fumaric acid is replaced with maleic acid of equal mass, other parameters are the same as those in Example 1.

[0034] Comparative Example 2: In step S1, except that ferric nitrate nonahydrate is replaced with ferric sulfate of equal mass, the other parameters are the same as those of Example 1.

[0035] Comparative Example 3: In step S1, except that ferric nitrate nonahydrate is replaced with ferrous nitrate of equal mass, the other parameters are the same as those in Example 1.

[0036] Example 2

[0037] S1. Preparation of porous MOF skeleton: 12 g of ferric nitrate nonahydrate and 3 g of fumaric acid were weighed and dissolved in 50 mL of distilled water. The mixture was stirred with a magnetic stirrer at 40 °C for 12 min. The mixture was then placed in a muffle furnace for high temperature treatment. The heating conditions were as follows: heating at 130 °C for 5 h, cooling and centrifuging to generate MIL-88 nanoparticles.

[0038] S2. Introducing cobalt into the MOF framework: Dissolve 1 g of the centrifuged MIL-88 particles and 2 g of cobalt nitrate hexahydrate in 50 mL of ethanol and treat in an oil bath at 100 °C for 1 h to obtain MIL-88@Co.

[0039] S3: The prepared MIL-88@Co nanoparticles were centrifuged at 4000r / min for 5min, then dried with anhydrous ethanol, and sintered in a tubular furnace under N2 atmosphere at a heating rate of 2℃ / min, 130℃ for 1h, and 350℃ for 2.5h to convert the cobalt element into cobalt tetroxide to obtain MIL-88@Co3O4;

[0040] S4, weigh 0.6g of magnesium sulfate and 0.5g of MIL-88@Co3O4, use a tubular furnace to reduce Co3O4 under hydrogen conditions and introduce magnesium ions to form MIL-88@CoMg, the reaction conditions are: 400℃, 2h;

[0041] S5: Use 3M hydrochloric acid and anhydrous ethanol to clean 0.8*1.0cm 2 The nickel foam base material is prepared by weighing 0.009 g of MIL-88@CoMg nanomaterial, 0.015 g of carbon powder, 0.05 mL of 0.1 mg / μL PTFE, and 5 mL of ethanol, and putting them into an ultrasonic cleaner for 30 min. After drying, the mixture is evenly applied to the treated nickel foam surface to obtain the MIL-88@CoMg hydrogen evolution catalytic material with nickel foam as the base material.

[0042] Comparative Example 4: In step S2, except that the cobalt nitrate hexahydrate is replaced with cobalt chloride of equal mass, the other parameters are the same as those of Example 2.

[0043] Comparative Example 5: In step S2, except that the cobalt nitrate hexahydrate is replaced with cobalt acetate of equal mass, the other parameters are the same as those in Example 2.

[0044] Comparative Example 6: In step S2, except that the cobalt nitrate hexahydrate is replaced with cobalt sulfate of equal mass, the other parameters are the same as those of Example 2.

[0045] Example 3

[0046] S1. Preparation of porous MOF skeleton: 15 g of ferric nitrate nonahydrate and 3 g of fumaric acid were weighed and dissolved in 50 mL of distilled water. The mixture was stirred with a magnetic stirrer at 70 °C for 15 min. The mixture was then placed in a muffle furnace for high temperature treatment. The heating conditions were as follows: heating at 120 °C for 7 h, cooling and centrifuging to generate MIL-88 nanoparticles.

[0047] S2. Introducing cobalt into the MOF framework: Dissolve 1 g of the centrifuged MIL-88 particles and 4 g of cobalt nitrate hexahydrate in 50 mL of ethanol and treat in an oil bath at 100 °C for 1 h to obtain MIL-88@Co.

[0048] S3: The prepared MIL-88@Co nanoparticles were centrifuged at 4000r / min for 5min, then dried with anhydrous ethanol, and sintered in a tubular furnace under N2 atmosphere at a heating rate of 2℃ / min, 130℃ for 1h, and 350℃ for 2.5h to convert the cobalt element into cobalt tetroxide to obtain MIL-88@Co3O4;

[0049] S4, weigh 0.4-1g of magnesium sulfate and 0.5g of MIL-88@Co3O4, use a tubular furnace to reduce Co3O4 under hydrogen conditions and introduce magnesium ions to form MIL-88@CoMg, the reaction conditions are: 400℃, 2h;

[0050] S5: Use 3M hydrochloric acid and anhydrous ethanol to clean 0.8*1.0cm 2 The nickel foam base material is prepared by weighing 0.01 g of MIL-88@Co Mg nanomaterial, 0.015 g of carbon powder, 0.05 mL of 0.1 mg / μL PTFE, and 5 mL of ethanol, and putting them into an ultrasonic cleaner for 30 min. After drying, the mixture is evenly applied to the treated nickel foam surface to obtain the MIL-88@CoMg hydrogen evolution catalytic material with nickel foam as the base material.

[0051] Comparative Example 7: In step S2, except that the cobalt nitrate hexahydrate is replaced with an equal mass of silver nitrate, the other parameters are the same as those in Example 3.

[0052] Comparative Example 8: In step S2, except that the cobalt nitrate hexahydrate is replaced with copper nitrate of equal mass, the other parameters are the same as those in Example 3.

[0053] Comparative Example 9: In step S2, except that the cobalt nitrate hexahydrate is replaced with ferrous nitrate of equal mass, the other parameters are the same as those in Example 3.

[0054] The catalyst electrodes for hydrogen evolution by electrolysis prepared in Examples 1-3 and Comparative Examples 1-9 were clamped by electrode racks so that the exposed portion was 0.8×0.8 cm 2 The square is used as the working electrode in the three-electrode system test. The prepared 1M KOH solution is used as the test electrolyte. Nitrogen is continuously introduced into the solution for 10 minutes to remove the dissolved air in the electrolyte. Then the prepared hydrogen evolution catalytic electrode is completely immersed in it. The main electrode in the three-electrode system is the Hg / HgO electrode, and the counter electrode is the platinum electrode. After the three electrodes are connected to the Shanghai Chenhua electrochemical workstation CHI660E, the electrolytic water hydrogen evolution catalytic reaction is started in the electrolyte, and the linear sweep voltammetry LSV performance curve of the catalyst is tested. The purpose of testing the LSV curve is to determine the catalytic activity of the catalyst. The test scan rate is 5mV s -1 , the voltage of the hydrogen evolution reaction is -2V-0V (vs.RHE), and the obtained potential is converted into the reversible hydrogen electrode potential according to the formula: E RHE =E Hg / HgO +0.098+0.059×pH, convert the obtained current into the current density per unit electrode area, and take the current density as 500mA cm -2 The corresponding over-potential is plotted and organized in a table. The test results are shown in Table 1 and Figure 3 As shown in Table 2, the current density value in the LSV curve is processed to obtain the Tafel slope curve. Figure 4 The voltage-time curve mainly tests the catalytic stability of the electrocatalyst. The electrolyte used in the durability test also uses 1M KOH solution. The test results are as follows: Figure 5 As shown; cyclic voltammetry CV was performed at room temperature at 20, 40, 60, 80, 100, 120, 140, 160, 180, and 200 mV s -1 The cyclic stability of the catalyst in Example 3 was tested at a scan rate of Figure 6 As shown, the double-layer capacitance curve of Example 3 can be obtained through data calculation, and the result is as follows Figure 7 .

[0055] Table 1 Test samples at a current density of 500 mA cm-2 The corresponding overpotential

[0056]

[0057]

[0058] Table 2 Tafel slope of test samples

[0059] Test samples <![CDATA[Tafel slope (mV dec -1 )]]> Example 1 43 Example 2 86 Example 3 69 Comparative Example 1 78 Comparative Example 2 73 Comparative Example 3 89 Comparative Example 4 87 Comparative Example 5 83 Comparative Example 6 91 Comparative Example 7 102 Comparative Example 8 106 Comparative Example 9 100

[0060] according to Figure 1 and Figure 2 It can be intuitively observed from the microstructure scanning images of Example 1 and Example 2 that the microstructure of the MIL-88@CoMg nanoparticles presents a nanorod structure. This ordered regular microstructure can increase the actual catalytic reaction area in the catalytic electrolysis of water. By introducing the structural regulation of the MOF pore skeleton and adding cobalt ions and magnesium ions to adjust the performance, the efficiency of catalytic hydrogen evolution can be improved.

[0061] Through Table 1 and Figure 3 The linear voltammetry data of the tested samples show that at the same 500 mA cm -2 Under the current density, the sample of Example 1 requires the lowest overpotential, which is only -0.550V. When comparing the hydrogen evolution catalytic performance of the examples with different material ratios, it can be seen that the material ratio of Example 1 is the most scientific and can achieve the best hydrogen evolution catalytic effect. On the other hand, in the comparative example, whether the raw materials of fumaric acid and ferric nitrate nonahydrate for preparing MIL-88 nanoparticles are changed or the addition of any one of cobalt ions and magnesium ions is changed, the catalytic performance cannot be improved, indicating that the MOF structural framework of MIL-88 and the synergistic effect of cobalt ions and magnesium ions play an important role in the catalysis of hydrogen evolution reaction; Observe Table 2 and Figure 4 It can be seen from the Tafel slope of the test samples that the Tafel slope of Example 1 is the smallest, which is 43 mV dec. -1 This indicates that the material with the smallest liquid junction resistance in Examples 1-3 and Comparative Examples 1-9 is Example 1, that is, the catalytic material of Example 1 has the best conductivity and can catalyze the electrolysis of water to produce more hydrogen energy under the same applied voltage.

[0062] Figure 5 The voltage-time curve of Example 1 was tested for 100 hours of hydrogen evolution reaction. It can be seen that during the catalytic hydrogen evolution reaction, Example 1 can maintain a substantially constant voltage, indicating that the stability of the reaction process is very good; Figure 6 The cyclic voltammetry curve of Example 3 shows that the -1 The scan rate was increased to 200 mV s -1During the scanning rate, the cyclic voltammetry curve has good closure, indicating that the catalytic hydrogen evolution reaction process of Example 3 is reversible, and the prepared hydrogen evolution catalytic material can be used repeatedly for a long time. Figure 7 The double layer capacitance of Example 3 is 20.38 mF cm -2 , indicating that the material has a good electrochemical specific surface area.

[0063] The above-mentioned embodiments only express the specific implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the protection scope of the present invention. It should be pointed out that, for those skilled in the art, without departing from the concept of the present invention, any other changes, modifications, substitutions, combinations, simplifications made without departing from the spirit and principle of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a MIL-88@CoMg water electrolysis hydrogen evolution catalyst based on nickel foam, specifically a hydrogen evolution catalyst containing iron, cobalt and magnesium, characterized in that: The preparation method is as follows: S1. Preparation of porous MOF skeleton: Weigh 10-15 parts of ferric nitrate nonahydrate and 3 parts of fumaric acid, dissolve them in 50 parts of distilled water, stir them with a magnetic stirrer at 30-70°C for 10-15 minutes, then put them in a muffle furnace, heat them at 120-150°C for 4-7 hours, cool them down and centrifuge them to generate MIL-88 nanoparticles; S2. Introducing cobalt into the MOF framework: Dissolve 1 part of the centrifuged MIL-88 particles and 1-4 parts of cobalt nitrate hexahydrate in 50 parts of ethanol, and treat in an oil bath at 100°C for 1 h to obtain MIL-88@Co; S3: The prepared MIL-88@Co nanoparticles were centrifuged at 4000r / min for 5min, then dried with anhydrous ethanol, and sintered in a tubular furnace under N2 atmosphere at a heating rate of 2℃ / min, 130℃ for 1h, and 350℃ for 2.5h to convert the cobalt element into cobalt tetroxide to obtain MIL-88@Co3O4; S4, weigh 0.4-1 parts of magnesium sulfate and 0.5 parts of MIL-88@Co3O4, use a tubular furnace to reduce Co3O4 under hydrogen conditions and introduce magnesium ions to form MIL-88@CoMg, the reaction conditions are: 400℃, 2h; S5: Use 3M hydrochloric acid and anhydrous ethanol to clean 0.8*1.0cm 2 The nickel foam base material is prepared by weighing 0.007-0.01 parts of MIL-88@CoMg nanomaterials, 0.015 parts of carbon powder, 0.05 parts of 0.1 mg / μL PTFE, and 5 parts of ethanol, and putting them into an ultrasonic cleaner for 30 minutes. After drying, the mixture is evenly applied to the treated nickel foam surface to obtain the MIL-88@CoMg hydrogen evolution catalyst based on nickel foam.

2. The method for preparing a MIL-88@CoMg water electrolysis hydrogen evolution catalyst based on nickel foam according to claim 1, characterized in that: The S1 weighed 10 g of ferric nitrate nonahydrate, 3 g of fumaric acid, and 50 mL of distilled water.

3. The method for preparing a MIL-88@CoMg water electrolysis hydrogen evolution catalyst based on nickel foam according to claim 1 or 2, characterized in that: The temperature of the muffle furnace in S1 is set to 150° C., and the heating time is 4 h.

4. The method for preparing a MIL-88@CoMg water electrolysis hydrogen evolution catalyst based on nickel foam according to claim 1, characterized in that: The S2 weighed cobalt nitrate hexahydrate is 1 g and ethanol is 50 mL.

5. The method for preparing a MIL-88@CoMg water electrolysis hydrogen evolution catalyst based on nickel foam according to claim 1, characterized in that: The magnesium sulfate weighed in S4 is 0.4 g.

6. The method for preparing a MIL-88@CoMg water electrolysis hydrogen evolution catalyst based on nickel foam as claimed in claim 1, characterized in that: The S5 weighed 0.007 g of MIL-88@CoMg nanomaterial, 0.015 g of carbon powder, 0.05 mL of 0.1 mg / μL PTFE, and 5 mL of ethanol.

7. The method for preparing a MIL-88@CoMg water electrolysis hydrogen evolution catalyst based on nickel foam according to claim 6, characterized in that: 0.01 parts of the MIL-88@CoMg nanomaterial weighed in S5.

8. A catalyst prepared by the preparation method mentioned in the preparation method of the MIL-88@CoMg water electrolysis hydrogen evolution catalyst based on nickel foam as claimed in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Preparation method of electrocatalytic material, corresponding material and use method

    CN112108149A

  • Metal-organic framework derived iron-nickel metal sulfide catalyst and preparation and application thereof

    CN112899723A

  • Preparation method of iron-based MOFs oxygen evolution electrocatalyst with high-activity crystal face proportion, and catalyst

    CN113073350A

  • Hollow metal organic framework-tannic acid-polypyrrole composite material as well as preparation method and application thereof

    CN113512735A

  • Nano ZnO / pyrolusite composite particle electrode and preparation method thereof

    CN114314762A