Antibacterial ceramic and preparation method thereof
By performing ion exchange and optimization processes on the ceramic surface, the silver ions distribution in the Ag+ area on the glaze layer surface is parabolic. Combined with pickling and alkali washing treatment, the problems of discoloration and insufficient antibacterial performance of antibacterial ceramic products are solved, and the problem of antibacterial ceramic products is improved Ceramics last and durable and reduce costs.
Patent Information
- Application Number
- CN202211310198.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-10-25
AI Technical Summary
Existing antibacterial ceramic products are prone to surface discoloration problems after ion exchange, and the antibacterial performance is insufficient and the cost is high.
By performing ion exchange on the ceramic surface, the glaze layer surface extends to the Ag+-containing area at a certain depth, adjust the silver ion concentration distribution curve to make it appear upward parabolic, and combine the pickling and alkali washing treatment steps to optimize the antibacterial molten salt components and Process, controlling the maximum distribution depth and content of silver ions in the glaze layer.
It effectively reduces the difference in color changes of ceramics after ion exchange, improves the sustainability and durability of antibacterial ceramics, maintains the antibacterial and wear resistance of the glaze surface, and reduces production costs.
Smart Images

Figure CN115536288B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of ceramic preparation, and in particular to an antibacterial ceramic and a preparation method thereof. Background Art
[0002] With the improvement of people's living standards and the development of science and technology, the emergence of SARS, H7N9, and now the new coronavirus, the importance of primary medical and health care is related to individuals, the country and even the entire world. People's requirements for hygiene and health are also getting higher and higher. The antibacterial ceramic products industry is gradually developing from the laboratory to the direction of daily use in people's livelihood.
[0003] The development of antibacterial ceramic technology, represented by INAX and TOTO, has gradually formed two major technical schools: metal ion doping preparation method and photocatalytic surface coating preparation method. Among them, the metal ion doping preparation method is to add metal ions such as silver and zinc to the glaze and then fire it through a firing process of 800-1380℃. The key lies in the preparation of antibacterial glaze, which not only requires that the antibacterial active ingredients in the antibacterial glaze are not destroyed after high-temperature firing at 800-1380℃ to ensure the realization of the antibacterial properties of the product. It is also required that the mechanical and thermodynamic properties of the antibacterial glaze can match the blank to ensure that the fired antibacterial ceramic products will not crack or be rough due to the mismatch of mechanical and thermodynamic properties. In addition, it is also necessary to ensure that the use of antibacterial glaze does not affect the color and appearance of ceramic products, and does not increase the production process of ceramic products, such as the number of sintering times, etc. However, this method is prone to reduce the volatilization of metal ions during high-temperature firing, and the cost of using metal ions is increased invisibly.
[0004] The photocatalytic surface coating preparation method is to coat a layer of TiO2 or TiO2 doped with metal ions sol-gel film on the surface of the finished ceramic product, and then sinter it at a low temperature (about 500°C). The key point is that after heat treatment, the film material is firmly bonded to the ceramic and maintains antibacterial properties. At present, there are a wide range of ceramic film preparation technologies and methods, mainly CVD, PVD, plasma sputtering deposition, and sol-gel (Sol-Gel) technologies. The coating method has a short-term antibacterial effect. After long-term use friction or steel wool wear resistance test, the antibacterial effect is greatly reduced.
[0005] In the preliminary study of the present invention, after preheating the basic white ceramic containing Na2O and K2O by ion exchange, the ceramic was placed in a mixed molten salt of molten copper sulfate, sodium sulfate and potassium sulfate for ion exchange, and cooled to obtain white antibacterial ceramic; copper ions were obtained on the surface of the ceramic, which had antibacterial properties, with an antibacterial activity value of R ≥ 3, and △E ≤ 1 before and after antibacterial. This technical solution has a high copper content in the molten salt, high ion exchange temperature requirements, and high production costs. This technical solution has an antibacterial △E ≤ 1 before and after antibacterial when the glaze is evenly applied. When preparing antibacterial ceramic products with uneven glaze thickness, discoloration problems caused by uneven glazing are still prone to occur. For example, the edge of the container mouth, the bottom of the container, and the bottom of the container are prone to discoloration due to less glazing in the ceramic container. Summary of the invention
[0006] The purpose of the present application is to provide an antibacterial ceramic and a preparation method thereof, which can solve to a certain extent the problem of discoloration of ceramic products after antibacterial ion exchange due to uneven surface glazing thickness.
[0007] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:
[0008] On the one hand, the present invention provides an antibacterial ceramic, including a body and a glaze layer arranged on the surface of the body. The antibacterial ceramic extends the surface of the glaze layer to a certain depth of Ag+-containing area through ion exchange. The ratio of the depth of the Ag+-containing area in the antibacterial ceramic to the thickness of the glaze layer on the surface of the ceramic body is 0.01-0.1. The color difference value △E of the antibacterial ceramic before and after ion exchange is ≤0.5 (this color difference value means extremely subtle color change and cannot be recognized by the naked eye).
[0009] Furthermore, the silver ion content in the antibacterial ceramic is 0.001-0.3wt%.
[0010] Furthermore, the maximum silver content of the antibacterial ceramic is 1.0-1.5at%, and the maximum value is distributed at a depth of 0.1-0.3% on the glaze layer surface (the ratio is the ratio of the depth from the glaze layer surface to the maximum value to the glaze layer thickness), and the glaze layer thickness is 0.1-0.3mm.
[0011] Furthermore, the antibacterial R value of the antibacterial ceramic is greater than 2.
[0012] Furthermore, the antibacterial ceramic has a rapid thermal change resistance temperature difference of ≥160°C.
[0013] Furthermore, the antibacterial ceramic surface is washed 500 times with a 5% concentration of sodium hypochlorite disinfectant, and the antibacterial rate is ≥99%.
[0014] In another aspect, the present invention provides a method for preparing an antibacterial ceramic, comprising the following steps:
[0015] Cleaning: put the base ceramic into pure water for cleaning;
[0016] Activation treatment, placing the cleaned base ceramic in an acid solution for soaking treatment, and then placing the base ceramic in an alkaline solution for alkaline soaking treatment;
[0017] Preheating treatment: placing the base ceramic in a preheating furnace for preheating;
[0018] Antibacterial treatment, placing the preheated base ceramic into molten antibacterial salt for antibacterial ion exchange treatment;
[0019] After cleaning, the base ceramic after antibacterial ion exchange is placed in a muffle furnace for cooling, and then cleaned with pure water.
[0020] Furthermore, acid polishing is performed after the acid solution immersion treatment and before the alkaline solution immersion treatment.
[0021] Furthermore, the acidic solution components are oxalic acid and water, wherein the concentration of oxalic acid is 0.6%-1.5%.
[0022] Furthermore, the acid solution is immersed for 1-5 minutes at a temperature of 60-80°C.
[0023] Furthermore, the alkaline solution is a sodium hydroxide aqueous solution with a pH of 11-12.
[0024] Furthermore, the soaking time of the alkaline solution is 3-10 minutes, and the temperature is 40-60°C.
[0025] Furthermore, the antibacterial molten salt is a nitrate composition containing silver, potassium and sodium, wherein the content of silver ions is 0.1%-5%.
[0026] Furthermore, the nitrate composition also contains lithium metal ions.
[0027] Furthermore, the antibacterial ion exchange temperature is controlled at the preheating temperature T1 and the molten salt temperature T2 and needs to be controlled so that T2-T1 is less than 50°C.
[0028] Furthermore, the molten salt temperature T2 is 350-440°C, preferably 360-400°C.
[0029] Furthermore, the antibacterial ion exchange time is controlled within 5-30 min, preferably 5-15 min.
[0030] Furthermore, the antibacterial molten salt is a nitrate composition containing silver, potassium and sodium metal ions, wherein the content of silver nitrate can be adjusted according to the content of feldspar in the ceramic glaze layer, and the mass ratio of feldspar in the glaze layer to silver nitrate is 10:1-2. The glaze is mainly composed of a mixture of feldspar, quartz, talc, kaolin, etc., and feldspar is divided into potassium feldspar, sodium feldspar, nepheline, lithium feldspar, etc. In the actual ion exchange process, silver ions and potassium ions in the molten salt are exchanged with sodium ions in the glaze layer. If the concentration of silver ions in the molten salt bath is too high, silver ions are preferentially exchanged with sodium ions due to their small radius and the close radius of silver and sodium ions, which will potentially form a higher silver content at a deeper penetration depth. In some cases, silver ions penetrate even deeper than potassium ions, and deeper silver ion penetration can cause discoloration of the glaze substrate. If the amount of silver ions in the molten salt bath is reduced to slow down the above effect, it means that there is less silver in the silver-containing area of the glaze layer, which will lead to reduced antibacterial efficiency or performance. In order to make the ion exchange efficient and fast, the content of silver nitrate in the molten salt can be adjusted by detecting the content of feldspar in the glaze layer. Therefore, by limiting such a relationship ratio, a better ion exchange effect can be obtained.
[0031] In addition, the sodium ion content in the glaze layer is closely related to the feldspar component of the glaze. Sodium, potassium, and silver are the main ions involved in antibacterial ion exchange. Excessive exchange of silver and potassium ions will cause the glaze performance to be reduced; if the sodium ion content in the glaze layer is too much, it will easily lead to a reduction in the mechanical properties of the ceramic glaze. If the sodium ion content in the glaze layer is low, the replaced potassium ions will be too saturated in the glass surface layer, which will cause microcracks to appear in the glass surface layer, and even under the action of external force, it is very easy to break. The present application controls the content of feldspar in the glaze surface layer and the silver ion content in the molten salt, without the need to add additional sodium nitrate to the molten salt, so that the glaze layer has both excellent antibacterial and long-lasting wear resistance.
[0032] The antibacterial ceramic provided in the first aspect of the present application optimizes the molten salt composition and process according to the glaze components so that the maximum silver content is distributed at a specific depth, and the Ag+ concentration distribution curve is an upward parabola. While meeting the antibacterial performance requirements, it can improve the sustainability and durability of the antibacterial effect and effectively reduce the redox discoloration problem caused by ion exchange.
[0033] The second aspect of the present application provides a method for preparing antibacterial ceramics, which adds acid washing and alkaline washing activation treatment steps before antibacterial ion exchange treatment. The acid washing removes heavy metal ions and inorganic salt deposits on the ceramic surface, which can cleanly and quickly remove metal impurities that may react with silver ions to change color. Alkaline washing is used to eliminate organic matter and microorganisms, and also eliminate factors that cause discoloration. By adding the antibacterial pre-treatment step, the difference in ceramic color change before and after antibacterial ion exchange can be effectively reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is the Ag content concentration curve of Example 9.
[0035] Figure 2 This is the Ag content concentration curve of Comparative Example 1. DETAILED DESCRIPTION
[0036] In order to explain the technical content, structural features, achieved objectives and effects of the technical solution in detail, the following is a detailed description in conjunction with specific embodiments.
[0037] In order to explain in detail the possible application scenarios, technical principles, specific schemes that can be implemented, and the purposes and effects that can be achieved, the following is a detailed description in conjunction with the specific embodiments listed. The embodiments described herein are only used to more clearly illustrate the technical solutions of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0038] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The term "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present application, as long as there is no technical contradiction or conflict, the various technical features mentioned in the embodiments can be combined in any way to form a corresponding implementable technical solution.
[0039] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.
[0040] In the description of this application, the term "and / or" is an expression used to describe the logical relationship between objects, indicating that three relationships may exist, for example, A and / or B, which means: A exists, B exists, and A and B exist at the same time. In addition, the character " / " in this article generally indicates that the objects before and after are in an "or" logical relationship.
[0041] In the present application, terms such as “first” and “second” are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship of quantity, priority or sequence between these entities or operations.
[0042] Without further limitations, in this application, the words "include", "comprises", "has" or other similar expressions used in the sentences are intended to cover non-exclusive inclusion. These expressions do not exclude the presence of additional elements in the process, method or product including the elements, so that the process, method or product including a series of elements may include not only those limited elements, but also other elements not explicitly listed, or also include elements inherent to such process, method or product.
[0043] Similar to the understanding in the Examination Guidelines, in this application, expressions such as "greater than", "less than", "exceed" and the like are understood to exclude the number itself; expressions such as "above", "below", "within" and the like are understood to include the number itself. In addition, in the description of the embodiments of this application, "multiple" means more than two (including two), and similar expressions related to "multiple" are also understood in this way, such as "multiple groups", "multiple times", etc., unless otherwise clearly and specifically limited.
[0044] As an inorganic non-metallic material, ceramic materials have many advantages such as high temperature resistance and corrosion resistance, and have been widely used in daily household, electronics, medical and other fields.
[0045] The inventors discovered in their research that the metal ions in the molten salt can be implanted into the ceramic glaze layer through the ion exchange process to obtain antibacterial properties. However, due to differences in the composition of various ceramic glazes, differences in the glaze layer structure, differences in the glazing process, and uneven glazing thickness in the process of preparing ceramic products, the ceramic surface with little or no glaze will change color after ion exchange.
[0046] In order to solve the above technical problems, the present application combines the glaze components through the first aspect to adjust and optimize the molten salt composition and process, so that the silver ion concentration distribution curve is an upward parabola, and the maximum value of the silver content is controlled in a specific depth range. While meeting the antibacterial performance requirements, it can improve the sustainability and durability of the antibacterial effect and effectively reduce the redox discoloration problem caused by ion exchange.
[0047] The second aspect of the present application provides a method for preparing antibacterial ceramics, which adds acid washing and alkaline washing activation treatment steps before antibacterial ion exchange treatment. Acid washing removes heavy metal ions and inorganic salt deposits on the ceramic surface, so that metal impurities that may react with silver ions to change color can be removed cleanly and quickly. Alkaline washing is used to eliminate organic matter and microorganisms, and also eliminates factors that cause discoloration. By adding the antibacterial pre-treatment step, the difference in color change of the ceramic before and after antibacterial ion exchange can be effectively reduced. The activation treatment order is acid washing first and then alkaline washing. If alkaline washing is performed first, heavy metal ions are easily precipitated, and the effect of acid washing is reduced.
[0048] Based on the above technical solution, the present application provides an embodiment of an antibacterial ceramic and a preparation method.
[0049] In some embodiments, the antibacterial ceramic extends the glaze layer surface to a certain depth of Ag+ containing region through ion exchange, and the ratio of the depth of the Ag+ containing region in the antibacterial ceramic to the thickness of the glaze layer on the surface of the ceramic body is 0.01-0.1. During the ion exchange process, the deeper the Ag+ diffusion depth, the easier it is to cause discoloration on the ceramic surface, and the deeper the Ag+ diffusion, the affected antibacterial effect, and also causes unnecessary cost waste.
[0050] In some embodiments, the color difference value △E of the antibacterial ceramic before and after ion exchange is ≤0.5. The ceramic is first tested for L*a*b* value according to QB / T1503-2011, and the ceramic after ion exchange is tested for L*a*b* value again, and △E is calculated, and the color difference is determined according to GB / T 3532-1995.
[0051] In some embodiments, the surface of the glaze layer extends to a certain depth of the Ag+ containing region, and the Ag+ concentration distribution curve formed in the region is parabolic upward, and the maximum value of the silver content in the Ag+ concentration distribution curve is 1.0-1.5at%, and the maximum value is distributed at a depth of 0.1-0.3% on the surface of the glaze layer. Among them, if the maximum value of the silver content is too high and the depth of the distribution is too deep, the antibacterial performance of the ceramic will deteriorate and discoloration may occur; and if the maximum value of the silver content is too low and the depth of the distribution is too shallow, the antibacterial performance of the ceramic will be poor, and the wear resistance and durability of the antibacterial effect will be unsatisfactory.
[0052] In some embodiments, after the acid solution immersion treatment, acid chemical polishing is performed before the alkaline solution immersion treatment to make the surface of the glaze layer smooth and uniform, remove the uneven texture of the ceramic surface, and enable it to maintain a certain range of pores to enhance the antibacterial effect.
[0053] Example
[0054] In order to further clearly explain and illustrate the technical solution of the present application, the following non-limiting examples are provided. The present application examples have been tried hard to ensure the accuracy of the numerical values, but some errors and deviations must be taken into account.
[0055] Preparation methods of antibacterial ceramics of Examples 1-10 and Comparative Examples 1-3:
[0056] Example 1
[0057] Wash the base ceramic in pure water;
[0058] The cleaned base ceramics were placed in a 0.8% oxalic acid solution for immersion treatment, the immersion time was 3 minutes, and the immersion temperature was 60°C;
[0059] Then, the base ceramic is immersed in a 10% sodium hydroxide aqueous solution for 3 minutes at a temperature of 60°C.
[0060] The base ceramic is placed in a preheating furnace for preheating at a temperature of 370°C for 11 minutes; the preheated base ceramic is placed in molten antibacterial salt for antibacterial ion exchange treatment at a temperature of 390°C for 10 minutes; the ceramic after antibacterial ion exchange is placed in a muffle furnace for cooling, and then washed with pure water to obtain antibacterial ceramics.
[0061] Example 2
[0062] Wash the base ceramic in pure water;
[0063] The cleaned base ceramics were placed in a 0.6% oxalic acid solution for immersion treatment, the immersion time was 5 minutes, and the immersion temperature was 70°C;
[0064] Then, the base ceramic is immersed in a 10% sodium hydroxide aqueous solution for 8 minutes at a temperature of 40°C.
[0065] The base ceramic is placed in a preheating furnace for preheating at 370°C for 11 minutes; the preheated base ceramic is placed in molten antibacterial salt for antibacterial ion exchange treatment at 400°C for 15 minutes; the ceramic after antibacterial ion exchange is placed in a muffle furnace for cooling, and then washed with pure water to obtain antibacterial ceramics.
[0066] Example 3
[0067] Wash the base ceramic in pure water;
[0068] The cleaned base ceramics were placed in a 0.8% oxalic acid solution for immersion treatment, the immersion time was 1 min, and the immersion temperature was 80°C;
[0069] Then, the base ceramic is immersed in a 15% sodium hydroxide aqueous solution for 6 minutes at a temperature of 50°C.
[0070] The base ceramic is placed in a preheating furnace for preheating at 390°C for 11 minutes; the preheated base ceramic is placed in molten antibacterial salt for antibacterial ion exchange treatment at 430°C for 8 minutes; the ceramic after antibacterial ion exchange is placed in a muffle furnace for cooling, and then washed with pure water to obtain antibacterial ceramics.
[0071] Example 4
[0072] Wash the base ceramic in pure water;
[0073] The cleaned base ceramics were placed in a 0.7% oxalic acid solution for immersion treatment, the immersion time was 3 minutes, and the immersion temperature was 60°C;
[0074] Then, the base ceramic is immersed in a 15% sodium hydroxide aqueous solution for 3 minutes at a temperature of 60°C.
[0075] The base ceramic is placed in a preheating furnace for preheating at 330°C for 10 minutes; the preheated base ceramic is placed in molten antibacterial salt for antibacterial ion exchange treatment at 360°C for 30 minutes; the ceramic after antibacterial ion exchange is placed in a muffle furnace for cooling, and then washed with pure water to obtain antibacterial ceramics.
[0076] Example 5
[0077] Wash the base ceramic in pure water;
[0078] The cleaned base ceramics were placed in a 1.5% oxalic acid solution for immersion treatment, the immersion time was 1 min, and the immersion temperature was 60°C;
[0079] Then, the base ceramic is immersed in a 15% sodium hydroxide aqueous solution for 10 minutes at a temperature of 50°C.
[0080] The base ceramic is placed in a preheating furnace for preheating at a temperature of 350°C for 15 minutes; the preheated base ceramic is placed in molten antibacterial salt for antibacterial ion exchange treatment at a temperature of 390°C for 25 minutes; the ceramic after antibacterial ion exchange is placed in a muffle furnace for cooling, and then washed with pure water to obtain antibacterial ceramics.
[0081] Example 6
[0082] Wash the base ceramic in pure water;
[0083] The cleaned base ceramics were placed in a 1.3% oxalic acid solution for immersion treatment, the immersion time was 1 min, and the immersion temperature was 60°C;
[0084] Then, the base ceramic is immersed in a 15% sodium hydroxide aqueous solution for 10 minutes at a temperature of 50°C.
[0085] The base ceramic is placed in a preheating furnace for preheating at 360°C for 15 minutes; the preheated base ceramic is placed in molten antibacterial salt for antibacterial ion exchange treatment at 400°C for 6 minutes; the ceramic after antibacterial ion exchange is placed in a muffle furnace for cooling, and then washed with pure water to obtain antibacterial ceramics.
[0086] Example 7
[0087] Wash the base ceramic in pure water;
[0088] The cleaned base ceramics were placed in a 1.0% oxalic acid solution for immersion treatment, the immersion time was 4 minutes, and the immersion temperature was 60°C;
[0089] Then, the base ceramic is immersed in a 15% sodium hydroxide aqueous solution for 10 minutes at a temperature of 40°C.
[0090] The base ceramic is placed in a preheating furnace for preheating at 360°C for 15 minutes; the preheated base ceramic is placed in molten antibacterial salt for antibacterial ion exchange treatment at 390°C for 5 minutes; the ceramic after antibacterial ion exchange is placed in a muffle furnace for cooling, and then washed with pure water to obtain antibacterial ceramics.
[0091] Example 8
[0092] Wash the base ceramic in pure water;
[0093] The cleaned base ceramics were placed in a 0.9% oxalic acid solution for immersion treatment, the immersion time was 5 minutes, and the immersion temperature was 60°C;
[0094] Then, the base ceramic is immersed in a 15% sodium hydroxide aqueous solution for 10 minutes at a temperature of 40°C.
[0095] The base ceramic is placed in a preheating furnace for preheating at 380°C for 15 minutes; the preheated base ceramic is placed in molten antibacterial salt for antibacterial ion exchange treatment at 410°C for 10 minutes; the ceramic after antibacterial ion exchange is placed in a muffle furnace for cooling, and then washed with pure water to obtain antibacterial ceramics.
[0096] Example 9
[0097] Wash the base ceramic in pure water;
[0098] The cleaned base ceramics were placed in a 0.9% oxalic acid solution for immersion treatment, the immersion time was 5 minutes, and the immersion temperature was 60°C;
[0099] Then, the base ceramic is immersed in a 15% sodium hydroxide aqueous solution for 10 minutes at a temperature of 40°C.
[0100] The base ceramic is placed in a preheating furnace for preheating at 360°C for 15 minutes; the preheated base ceramic is placed in molten antibacterial salt for antibacterial ion exchange treatment at 390°C for 6 minutes; the ceramic after antibacterial ion exchange is placed in a muffle furnace for cooling, and then washed with pure water to obtain antibacterial ceramics.
[0101] Example 10
[0102] Wash the base ceramic in pure water;
[0103] The cleaned base ceramics were placed in a 0.9% oxalic acid solution for immersion treatment, the immersion time was 5 minutes, and the immersion temperature was 60°C;
[0104] Then, the base ceramic is immersed in a solution containing 2% hydrofluoric acid, 8% nitric acid, and the balance water for 5 minutes at a temperature of 60°C;
[0105] Then, the base ceramic is immersed in a 15% sodium hydroxide aqueous solution for 10 minutes at a temperature of 40°C.
[0106] The base ceramic is placed in a preheating furnace for preheating at a temperature of 340°C for 5 minutes; the preheated base ceramic is placed in molten antibacterial salt for antibacterial ion exchange treatment at a temperature of 380°C for 6 minutes; the ceramic after antibacterial ion exchange is placed in a muffle furnace for cooling, and then washed with pure water to obtain antibacterial ceramics.
[0107] Comparative Example 1
[0108] Wash the base ceramic in pure water;
[0109] The base ceramic is placed in a preheating furnace for preheating at a temperature of 350°C for 15 minutes; the preheated base ceramic is placed in molten antibacterial salt for antibacterial ion exchange treatment at a temperature of 450°C for 20 minutes; the ceramic after antibacterial ion exchange is placed in a muffle furnace for cooling, and then washed with pure water to obtain antibacterial ceramics.
[0110] Comparative Example 2
[0111] Wash the base ceramic in pure water;
[0112] The cleaned base ceramics were placed in a 0.9% oxalic acid aqueous solution for immersion treatment, the immersion time was 5 minutes, and the immersion temperature was 60°C;
[0113] The base ceramic is placed in a preheating furnace for preheating at 320°C for 15 minutes; the preheated base ceramic is placed in molten antibacterial salt for antibacterial ion exchange treatment at 400°C for 30 minutes; the ceramic after antibacterial ion exchange is placed in a muffle furnace for cooling, and then washed with pure water to obtain antibacterial ceramics.
[0114] Comparative Example 3
[0115] Wash the base ceramic in pure water;
[0116] Then, the base ceramic is immersed in a 15% sodium hydroxide aqueous solution for 10 minutes at a temperature of 40°C.
[0117] The base ceramic is placed in a preheating furnace for preheating at a temperature of 330°C for 15 minutes; the preheated base ceramic is placed in molten antibacterial salt for antibacterial ion exchange treatment at a temperature of 420°C for 25 minutes; the ceramic after antibacterial ion exchange is placed in a muffle furnace for cooling, and after cooling, it is washed with pure water to finally obtain antibacterial ceramics.
[0118] Surface glaze layer components: The components and contents of the glaze surface layer were measured using the ARLTM PERFORM'X X-ray fluorescence spectrometer (XRF) produced by Thermo Fisher Scientific. The measurement parameters were: voltage 60 kV, current 40 mA;
[0119] Contains Ag + Depth of the region (μm): The depth of antibacterial ion implantation was detected using an IMS 7f secondary ion mass spectrometer (SIMS) produced by CAMECA;
[0120] Antimicrobial effective value (R): Escherichia coli ATCC8739 and Staphylococcus aureus ATCC6538P were tested using the JIS Z 2801:2010 test method;
[0121] Ag concentration: X-ray photoluminescence spectroscopy (XPS) was used to measure the Ag concentration at each layer depth (nanometer level), and the results were recorded as atomic percentages.
[0122] Antibacterial rate after cleaning with 5% sodium hypochlorite: tested using the JC / 897-2014 testing method.
[0123] Color difference △E after antibacterial treatment: The base ceramics are first tested for L*a*b* values according to QB / T 1503-2011, and the antibacterial ceramics after ion exchange are tested for L*a*b* values, and △E is calculated, and the color difference is determined according to GB / T 3532-1995.
[0124] Resistance to sudden thermal changes: Test by cycling 10 times between 10°C and 200°C to see if there are cracks or other defects.
[0125] Table 1 shows the antibacterial molten salt components and related performance parameters of each embodiment and comparative example
[0126]
[0127]
[0128]
[0129] Performance result description: It can be seen from the above examples combined with Table 1 that the antibacterial ceramics prepared in Examples 1-10 extend the glaze layer surface to a certain depth of Ag+-containing area through ion exchange, and the ratio of the depth of the Ag+-containing area in the antibacterial ceramic to the thickness of the glaze layer on the surface of the ceramic embryo is 0.01-0.1: 1. During the ion exchange process, the deeper the Ag+ diffusion depth, the easier it is to cause discoloration on the ceramic surface, and the deeper the Ag+ diffusion, the more it will affect the antibacterial effect, and also cause unnecessary cost waste.
[0130] The basic ceramic is subjected to ion exchange through the activation treatment in the embodiment combined with the optimized antibacterial molten salt, and the color difference value before and after △E≤0.5. This technical solution enables the ceramic glaze to maintain a certain content of silver ions. The control of the concentration content makes the ceramic glaze have effective antibacterial properties and can avoid discoloration and cost waste due to the deep diffusion of excessive silver ions.
[0131] The antibacterial molten salt is a nitrate composition containing silver, potassium and sodium, in which the content of silver nitrate can be adjusted according to the content of feldspar in the ceramic glaze layer. Feldspar is an aluminum silicate mineral containing calcium, sodium and potassium. Its content promotes the rate of ion exchange and metal ion diffusion of ceramic glaze. However, excessive implantation and diffusion will have a negative effect on the antibacterial properties and color of the glaze. Therefore, the mass ratio of feldspar in the glaze layer: silver nitrate is best between 10:1-2.
[0132] While the antibacterial ion exchange is taking place on the glaze surface, the ion exchange between K / Na or Na / Li is also carried out on the glaze surface, forming a compressive stress layer on the glaze surface to improve the surface strength of the ceramic product and the resistance of the ceramic to rapid thermal changes and temperature differences.
[0133] It can be seen from the combination of Examples 9 and 10 that adding a certain amount of lithium nitrate to the antibacterial molten salt can promote the effect of accelerating ion exchange. Immersion in a lithium ion-containing metal salt will cause ion exchange between the sodium ions in the glaze layer and the lithium ions in the metal salt. The lithium ions with a small radius have a fast replacement diffusion rate and are more easily implanted into the surface layer of the glaze layer, causing changes in the spatial structure of the glaze surface, reducing steric hindrance, and promoting the exchange of antibacterial silver ions with a larger radius. At the same time, due to the reduction of steric hindrance, the energy required for the antibacterial metal ions to perform ion exchange in the glaze layer is reduced. Therefore, the temperature and / or time of the ion exchange can be further reduced. In addition, there are many factors that affect the time and temperature of ion exchange, such as the alkali metal content of the ion exchange object, the concentration formula of the ion exchange molten salt, etc.
[0134] By combining the embodiments and comparative examples, it can be seen that comparative examples 1-3 did not undergo activation acid-base treatment or only performed one step, and the ratio of feldspar to silver nitrate in the glaze layer was not between 10:1-2, which resulted in the silver concentration diffusing to a deeper level, causing the silver ions to form silver colloid or the silver ions to undergo oxidation-reduction reactions with metal ions, inorganic salts or organic matter in the ceramic, resulting in a color difference △E value on the surface higher than 0.5, and an obviously uneven yellow color visible to the naked eye. In addition, the difference between the preheating temperature and the ion exchange temperature in the comparative example was large, and some crack defects appeared on the surface.
[0135] Table 2 shows the relevant performance parameters of Examples 1, 3, 5, 9 and Comparative Example 1
[0136]
[0137] Performance result description: From the above embodiment combined with Table 2, it can be seen through XPS detection that the antibacterial ceramic extends the glaze surface to a certain depth of Ag+ containing area through ion exchange, and the Ag+ concentration distribution curve formed in this area is an upward parabola. In the Ag+ concentration distribution curve, the maximum value of the silver content is 1.0-1.5at%, and the maximum value is distributed at the depth of 0.1-0.3% on the surface of the glaze layer. According to the embodiment, it can be seen that the maximum value of the silver content is distributed in the range of 300-700nm. The highest concentration in this range can obtain effective antibacterial performance and wear resistance, and keep the color difference △E <0.5 after the antibacterial ion exchange of the ceramic glaze. The maximum value of comparative example 1 is distributed at a depth of about 5000nm. It can be seen from the above test that the maximum value of the silver content is too high and the depth of distribution is too deep, which will cause the antibacterial performance of the ceramic to deteriorate and the possibility of discoloration; while the maximum value of the silver content is too low and the depth of distribution is too shallow, which will cause the antibacterial performance of the ceramic to be poor, and the wear resistance and durability of the antibacterial effect are not ideal.
[0138] Further comparison with the comparative example shows that the comparative example has a lower surface silver ion content (the surface silver ion content is detected by XPS or secondary ion mass spectrometry (SIMS) to detect the antibacterial ion implantation depth (the detection depth is in the range of 10-20 nm). Most of the silver ion content is implanted deeper. Although it also has a certain content of silver ions, due to process differences, excessively high temperature or high concentration of silver, silver colloidization will occur, and the prepared ceramic has a poor antibacterial effect, and silver colloidization will cause an obvious yellow color.
[0139] The ceramics of the embodiment are activated before ion exchange, wherein acid washing reduces the deposition of heavy metal ions and inorganic salts on the glaze layer and the surface of the ceramic body, so that metal impurities that may react with silver ions to change color can be removed cleanly and quickly, and alkaline washing is used to eliminate organic matter and microorganisms, and also eliminate factors that cause discoloration. Furthermore, by controlling the concentration of silver ions in the ion exchange, the discoloration of the ceramic surface caused by uneven glazing thickness can be effectively prevented, and the color difference △E after antibacterial treatment is controlled to be less than 0.5.
[0140] The ceramic glaze of the embodiment maintains an effective silver concentration within a certain depth range on the surface, and after 500 cleanings with a 5% sodium hypochlorite solution, it still maintains an antibacterial rate of ≥99.9. The comparative example has poor surface antibacterial performance due to the excessively deep distribution of the silver concentration.
[0141] The above description is only an implementation mode of the present invention, and does not limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made by using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing an antibacterial ceramic, the antibacterial ceramic comprising a body and a glaze layer arranged on the surface of the body, characterized in that: The antibacterial ceramics are provided with Ag-containing glaze extending from the surface of the glaze layer to a certain depth inside by ion exchange. + The region containing Ag + The ratio of the depth of the region to the thickness of the glaze layer is 0.01-0.1:1, and the color difference value of the antibacterial ceramic before and after ion exchange is △E≤0.5; the antibacterial molten salt is a nitrate composition containing silver, potassium and sodium, and the nitrate composition also contains lithium metal ions; the content of silver nitrate is adjusted according to the content of feldspar in the ceramic glaze layer, and the mass ratio of feldspar in the glaze layer to silver nitrate is 10:1-2; The silver ion content in the antibacterial ceramic is 0.001-0.3wt%, calculated based on the total weight of the glaze layer; The preparation method comprises the following steps: (1) Cleaning: Place the base ceramic in pure water for cleaning; (2) Activation treatment: the cleaned base ceramic is placed in an acid solution for soaking treatment, and then the base ceramic is placed in an alkaline solution for soaking treatment; (3) Preheating treatment: Place the base ceramic in a preheating furnace for preheating; (4) Antibacterial treatment: placing the preheated base ceramic into molten antibacterial molten salt for antibacterial ion exchange treatment; (5) Cleaning: The ceramic after antibacterial ion exchange is placed in a muffle furnace for cooling, and then cleaned with pure water; The acidic solution in step (2) is an aqueous solution of oxalic acid with a mass concentration of 0.6%-1.5%; The immersion time of the acid solution in step (2) is 1-5 minutes, and the temperature is 60-80°C; The alkaline solution in step (2) is a sodium hydroxide aqueous solution having a pH of 11-12; The immersion time of the alkaline solution in step (2) is 3-10 minutes, and the temperature is 40-60°C.
2. The method for preparing the antibacterial ceramic according to claim 1, characterized in that: The Ag-containing + The distribution of silver content in the region is parabolic upward, with a maximum value of 1.0-1.5at%, and the maximum value is distributed from the surface of the glaze layer to a depth of 0.1-0.3%.
3. The method for preparing the antibacterial ceramic according to claim 1, characterized in that: The antibacterial molten salt in step (4) has a silver ion content of 0.1wt%-5wt%.
4. The method for preparing the antibacterial ceramic according to claim 1, characterized in that: The relationship between the preheating temperature T1 in step (3) and the temperature T2 of the antibacterial molten salt in step (4) is: T2-T1<50°C.
5. The method for preparing the antibacterial ceramic according to claim 1, characterized in that: The time of the antibacterial ion exchange in step (4) is controlled within 5-30 minutes.
Citation Information
Patent Citations
Antimicrobial article with functional coating and methods for making the antimicrobial article
CN106458703A
Antimicrobial articles and methods of making and using same
CN111094207A
White antibacterial ceramic and preparation method thereof
CN112830813A
Antibacterial ceramic and preparation method thereof
CN113716976A
Antibacterial tempered glass and preparation method thereof
CN113816619A