Zinc-aluminum-magnesium coating, zinc-aluminum-magnesium coating steel plate and preparation method thereof

By adding Si to the zinc-aluminum-magnesium coating to form Mg-Si compound particles and a surface oxide film, the problem of high surface friction factor of the zinc-aluminum-magnesium coating steel plate is solved, excellent lubrication performance and corrosion resistance are achieved, and additional lubrication is avoided. Processing and cost savings.

CN115572932BActive Publication Date: 2024-10-18SHOUGANG GROUP CO LTD +1

Patent Information

Application Number
CN202211124328.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-15
Publication Date
2024-10-18
Estimated Expiration
2042-09-15

AI Technical Summary

Technical Problem

The surface friction coefficient of the existing zinc-aluminum-magnesium coated steel plate is high, resulting in poor lubrication performance and difficulty in meeting complex processing requirements.

Method used

Si element is added to the zinc-aluminum-magnesium coating to form no less than 0.01% Mg-Si compound particles with a particle size of ≤5um, which are embedded in the surface of the coating to form a hard phase, reduce frictional resistance, and form 1-50nm on the surface. Oxide film reduces friction coefficient in point contact state.

Benefits of technology

Significantly reduces the frictional resistance on the surface of zinc-aluminum-magnesium coating, improves lubrication performance, avoids the operation of conventional lubrication treatment, saves production costs, and maintains excellent corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115572932B_ABST
    Figure CN115572932B_ABST
Patent Text Reader

Abstract

The present invention provides a zinc-aluminum-magnesium coating, a zinc-aluminum-magnesium coated steel sheet and a preparation method thereof, belonging to the field of coating technology. The zinc-aluminum-magnesium coating comprises the following components: Al, Mg, Si, Zn and impurities from preparing the zinc-aluminum-magnesium coating; in terms of volume fraction, the surface of the zinc-aluminum-magnesium coating contains no less than 0.01% of Mg-Si compound particles, and the size of the Mg-Si compound particles is ≤5um. The Si in the coating can form Mg-Si compound particles with the Mg in the coating, and the size of the Mg-Si compound particles is ≤5um, which can be embedded in the coating surface and become a hard phase in the friction process, so that the friction process presents a point contact state, and significantly reduces the friction resistance on the surface of the zinc-aluminum-magnesium coating; when applied to the zinc-aluminum-magnesium coated steel sheet, the surface of the zinc-aluminum-magnesium coated steel sheet has excellent lubrication performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of coating and plating technology, and in particular to a zinc-aluminum-magnesium coating, a zinc-aluminum-magnesium coated steel plate and a preparation method thereof. Background Art

[0002] Hot-dip galvanized aluminum-magnesium coated steel sheet is a new type of high corrosion resistant hot-dip alloy coated steel sheet. This coating is based on the traditional pure zinc coating, with magnesium and aluminum added to the coating, which significantly improves the flat corrosion resistance and cut corrosion resistance of the coating. It can be widely used in the manufacture of automobiles, home appliances, steel structures, etc. with high corrosion resistance requirements.

[0003] At present, the surface friction coefficient of the existing zinc-aluminum-magnesium coated steel plate is relatively high, which makes its surface lubrication performance poor. Summary of the invention

[0004] The embodiments of the present application provide a zinc-aluminum-magnesium coating, a zinc-aluminum-magnesium coated steel plate and a preparation method thereof to solve the technical problem that the surface friction coefficient of the existing zinc-aluminum-magnesium coated steel plate is high, resulting in poor surface lubrication performance.

[0005] In a first aspect, an embodiment of the present application provides a zinc-aluminum-magnesium coating, wherein the zinc-aluminum-magnesium coating comprises the following components:

[0006] Al, Mg, Si, Zn and impurities from preparing the zinc-aluminum-magnesium coating;

[0007] Calculated by volume fraction, the surface of the zinc-aluminum-magnesium coating contains no less than 0.01% of Mg-Si compound particles, and the size of the Mg-Si compound particles is ≤5um.

[0008] Furthermore, the zinc-aluminum-magnesium coating comprises the following components by mass fraction:

[0009] Al: 1-8%; Mg: 1-4%; Si: 0.001-0.1%; the rest is Zn and impurities from preparing the zinc-aluminum-magnesium coating.

[0010] Furthermore, the surface of the zinc-aluminum-magnesium coating contains an oxide layer with a thickness of 1-50 nm.

[0011] Furthermore, the oxide includes at least one of Al oxide, Mg oxide and Zn oxide.

[0012] Furthermore, in terms of mass fraction, the Mg element in the oxide is ≥ 10%, and / or the Al element in the oxide is ≥ 10%.

[0013] Furthermore, in terms of mass fraction, the Si element content in the zinc-aluminum-magnesium coated steel plate coating does not exceed one twentieth of the Mg element content.

[0014] Furthermore, the surface friction coefficient of the zinc-aluminum-magnesium coating is ≤0.005.

[0015] In a second aspect, an embodiment of the present application provides a zinc-aluminum-magnesium coated steel plate, wherein the zinc-aluminum-magnesium coated steel plate comprises a steel plate substrate and a coating attached to the surface of the steel plate substrate;

[0016] The coating is the zinc-aluminum-magnesium coating described in the first aspect.

[0017] In a third aspect, an embodiment of the present application provides a method for preparing the zinc-aluminum-magnesium coated steel sheet according to the second aspect, the preparation method comprising:

[0018] Obtaining a steel plate substrate to be coated with a zinc-aluminum-magnesium coating;

[0019] The steel plate substrate is hot-dip plated, then annealed, cooled, skin-passed and coiled to obtain a zinc-aluminum-magnesium coated steel plate;

[0020] Wherein, the hot dip plating solution comprises the following components by mass fraction:

[0021] Al: 1-8%; Mg: 1-4%; Si: 0.001-0.1%; the rest is Zn and inevitable impurities.

[0022] Furthermore, the annealing process parameters include: a temperature of 120° C. to 320° C., a time of 10s to 60s, and a molar fraction of oxygen molecules in the annealing atmosphere of 10% to 50%.

[0023] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0024] The embodiment of the present application provides a zinc-aluminum-magnesium coating, in which the Si in the coating can form no less than 0.01% of Mg-Si compound particles with the Mg in the coating, and the size of the Mg-Si compound particles is ≤5um, and can be embedded in the surface of the coating to become a hard phase in the friction process, so that the friction process presents a point contact state, significantly reducing the friction resistance on the surface of the zinc-aluminum-magnesium coating; when applied to zinc-aluminum-magnesium coated steel plates, the surface of the zinc-aluminum-magnesium coated steel plates has excellent lubrication properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0027] Figure 1 A schematic flow chart of a method for preparing a zinc-aluminum-magnesium coated steel plate provided in an embodiment of the present application;

[0028] Figure 2 This is a microstructure diagram of the zinc-aluminum-magnesium coating in a zinc-aluminum-magnesium coated steel plate provided in an embodiment of the present application. DETAILED DESCRIPTION

[0029] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are for illustrating the present invention, rather than limiting the present invention.

[0030] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.

[0031] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0032] Hot-dip galvanized aluminum-magnesium coated steel sheet is a new type of high corrosion resistant hot-dip alloy coated steel sheet. This coating is based on the traditional pure zinc coating, with magnesium and aluminum added to the coating, which significantly improves the flat corrosion resistance and cut corrosion resistance of the coating. It can be widely used in the manufacture of automobiles, home appliances, steel structures, etc. with high corrosion resistance requirements.

[0033] At present, the surface friction coefficient of the existing zinc-aluminum-magnesium coated steel plate is relatively high, which makes its surface lubrication performance poor. However, in order to further meet certain complex processing requirements, it is necessary to lubricate the surface to reduce the friction coefficient of the coating surface. Conventional lubrication treatment is to form a chemical film on the surface, including organic film and inorganic film. However, the bonding force between this film and the coating is poor and it is easy to peel off during processing. At the same time, the formation of the surface chemical film requires the use of special chemicals, which has certain harm to the environment.

[0034] The technical solution provided by the embodiment of the present invention is to solve the above technical problems, and the overall idea is as follows:

[0035] In a first aspect, an embodiment of the present application provides a zinc-aluminum-magnesium coating, wherein the zinc-aluminum-magnesium coating comprises the following components:

[0036] Al, Mg, Si, Zn and impurities from preparing the zinc-aluminum-magnesium coating;

[0037] Calculated by volume fraction, the surface of the zinc-aluminum-magnesium coating contains no less than 0.01% of Mg-Si compound particles, and the size of the Mg-Si compound particles is ≤5um.

[0038] The embodiment of the present application provides a zinc-aluminum-magnesium coating, in which Si in the coating can form no less than 0.01% of Mg-Si compound particles with Mg in the coating, and the size of the Mg-Si compound particles is ≤5um, and can be embedded in the surface of the coating to become a hard phase in the friction process, so that the friction process presents a point contact state, significantly reducing the surface friction resistance of the zinc-aluminum-magnesium coating; when applied to zinc-aluminum-magnesium coated steel plates, the surface of the zinc-aluminum-magnesium coated steel plates has excellent lubrication properties, while avoiding the operation of lubrication treatment of the surface of the zinc-aluminum-magnesium coated steel plates, saving production costs.

[0039] In the present application, the "Mg-Si compound" specifically refers to the intermetallic compound Mg2Si formed by Mg and Si, which has a melting point of 1085°C and a cubic crystal form.

[0040] As an implementation method of an embodiment of the present invention, the zinc-aluminum-magnesium coating includes the following components by mass fraction:

[0041] Al: 1-8%; Mg: 1-4%; Si: 0.001-0.1%; the rest is Zn and impurities from preparing the zinc-aluminum-magnesium coating.

[0042] The design principles of the elements and dosages of the zinc-aluminum-magnesium coating in this application are as follows:

[0043] Al: In the production of hot-dip galvanized aluminum-magnesium coated steel sheets, in order to ensure that the coated steel sheets have excellent corrosion resistance, more than 1% Al is usually added to the coating. As the concentration of Al increases, the reaction between the steel sheet and Al during hot-dip coating is significantly accelerated, making it easy to form a thicker inhibition layer. This thicker inhibition layer increases the brittleness of the inhibition layer itself. This makes it easy for cracks to appear inside the inhibition layer of the hot-dip galvanized aluminum-magnesium coating during the friction process, resulting in fracture from the inside of the inhibition layer, causing the coating to peel off and increase friction resistance. Therefore, the Al content in the present invention is controlled to be 1-8%.

[0044] Mg: The Mg element in the hot-dip galvanized aluminum-magnesium coating can significantly improve the corrosion resistance of the coating. Generally speaking, the Mg content is not less than 1% to have obvious corrosion resistance benefits. However, when the Mg content in the coating is too high, a large number of large-sized Mg-containing compounds will appear in the coating. Such Mg-containing compounds are usually brittle phases, which are prone to brittle fracture during surface friction and increase friction resistance. Therefore, the Mg content is controlled to 1-4% in the present invention.

[0045] Si: A certain amount of Si element needs to be added to the hot-dip zinc-aluminum-magnesium coating. Si is also an element that is easy to combine with steel plates and has a high solubility in the Fe-Al inhibition layer. After Si dissolves in the Fe-Al inhibition layer, it can strengthen the inhibition layer and improve the strength of the inhibition layer. At the same time, the dissolution of Si in the inhibition layer can also prevent the inhibition layer from growing too fast during hot-dip plating, avoiding excessive growth of the inhibition layer. Silicon is a high-melting-point metal that can form high-melting-point intermetallic compounds with other metals in the alloy liquid. As a nucleation core during the solidification of the coating, it plays a role in refining the grains of the zinc-aluminum-magnesium coating, making it difficult for the coating surface to peel off during the friction process, thereby reducing the friction factor. In addition, Si in the coating can form Mg-Si compound particles with Mg in the coating. When the size of such Mg-Si compound particles is small, they can be embedded in the surface of the coating and become a hard phase in the friction process, making the friction process present a point contact state and reducing friction resistance. Therefore, the amount of Si element added is usually not less than 0.001%, so as to ensure that the volume fraction of the Mg-Si phase on the surface of the coating will not be too small. However, if the Si content is too high, large particles of Mg-Si compounds will be formed, which will deteriorate the toughness of the coating, making the coating prone to cracking and peeling during friction, thereby increasing friction resistance. Therefore, in the present invention, Si is controlled to 0.001-0.1%.

[0046] As an implementation method of the embodiment of the present invention, the surface of the zinc-aluminum-magnesium coating contains an oxide layer with a thickness of 1-50 nm.

[0047] In the present application, there is also a layer of oxide on the surface of the zinc-aluminum-magnesium coating. The oxide is mainly an oxide of Al, Mg, and Zn. The thickness of this oxide is only 1-50nm. Although the hardness is higher than that of the coating, the toughness is relatively poor. Therefore, during the friction process, the oxide film will quickly break into fine dispersed particles, which are distributed between the friction pair and the coating to form a medium that can flow, so that there is no direct physical contact between the friction pair and the coating, thereby further significantly reducing the friction factor. If this oxide film is too thin, it is obviously impossible to form enough fine dispersed particles and achieve no lubrication effect. However, if the oxide layer is too thick, although it will break during friction, it is difficult to form sufficiently fine particles, but it is easy to form a lamellar oxide film. This oxide film will wrap around the surface of the friction pair and cannot achieve the effect of flowing medium lubrication.

[0048] As an implementation of an embodiment of the present invention, the oxide includes at least one of an oxide of Al, an oxide of Mg and an oxide of Zn.

[0049] As an implementation manner of the embodiment of the present invention, in terms of mass fraction, the Mg element in the oxide is ≥ 10%, and / or the Al element in the oxide is ≥ 10%.

[0050] In the present application, the oxide should be mainly composed of Mg and Al oxides, because the toughness of the two oxides of Mg and Al is lower and they are more likely to form fine oxide particles under friction conditions. Therefore, the mass fraction of Mg element in the surface oxide is not less than 10%, and the mass fraction of Al element is not less than 10%.

[0051] As an implementation method of an embodiment of the present invention, the Si element content in the zinc-aluminum-magnesium coated steel plate coating does not exceed one twentieth of the Mg element content, measured by mass fraction.

[0052] In the present application, it is required that the Si content in the coating does not exceed one twentieth of the Mg content in the coating, so as to avoid the presence of large particles of Mg-Si compounds in the coating.

[0053] As an implementation method of the embodiment of the present invention, the surface friction coefficient of the zinc-aluminum-magnesium coating is ≤0.005.

[0054] The zinc-aluminum-magnesium coating provided by the present application has a low surface friction coefficient and does not require conventional lubrication treatment such as forming a chemical film on the surface, thereby saving production costs; at the same time, it has excellent corrosion resistance.

[0055] In a second aspect, an embodiment of the present application provides a zinc-aluminum-magnesium coated steel plate, wherein the zinc-aluminum-magnesium coated steel plate comprises a steel plate substrate and a coating attached to the surface of the steel plate substrate;

[0056] The coating is the zinc-aluminum-magnesium coating described in the first aspect.

[0057] The zinc-aluminum-magnesium coated steel plate provided in the present application adopts the zinc-aluminum-magnesium coating described in the first aspect as the coating, so the zinc-aluminum-magnesium coated steel plate has excellent surface lubrication and corrosion resistance.

[0058] In a third aspect, an embodiment of the present application provides a method for preparing the zinc-aluminum-magnesium coated steel sheet according to the second aspect, the preparation method comprising:

[0059] Obtaining a steel plate substrate to be coated with a zinc-aluminum-magnesium coating;

[0060] The steel plate substrate is hot-dip plated, then annealed, cooled, skin-passed and coiled to obtain a zinc-aluminum-magnesium coated steel plate;

[0061] Wherein, the hot dip plating solution comprises the following components by mass fraction:

[0062] Al: 1-8%; Mg: 1-4%; Si: 0.001-0.1%; the rest is Zn and inevitable impurities.

[0063] In the present application, the steel plate substrate to be coated with zinc, aluminum and magnesium can be obtained by conventional steel preparation process or directly adopt commercially available steel plate substrate, the conventional steel preparation process includes: first heating the slab, then rough rolling and finishing rolling to obtain hot rolled plate, then coiling the hot rolled plate into hot rolled coil and cooling, cold rolling the hot rolled coil to obtain cold hard coil, and continuous annealing to obtain the steel plate substrate to be coated with zinc, aluminum and magnesium. This application document will not repeat it.

[0064] In the present application, hot-dip plating is to hot-dip the steel plate substrate to be plated with zinc-aluminum-magnesium coating in a plating solution containing Al: 1-8%, Mg: 1-4%, Si: 0.001-0.1%, and the rest is Zn and unavoidable impurity elements, and then take it out. The remaining operation steps of hot-dip plating in the present application are carried out according to conventional hot-dip plating, and this application document will not repeat them.

[0065] As an implementation method of the present invention, the steel plate substrate is annealed after hot-dip galvanizing, and the annealing process parameters include: temperature of 120°C to 320°C, time of 10s to 60s, and the molar fraction of oxygen molecules in the annealing atmosphere of 10% to 50%.

[0066] In the present application, the purpose of annealing the steel plate substrate after hot-dip plating is: the first purpose is to diffuse the Al and Mg elements in the coating to the surface of the coating through annealing treatment, and react with the oxygen molecules in the annealing atmosphere to form an oxide film rich in Mg and Al. The second purpose is to combine Mg and Si in the coating with each other through annealing treatment to form Mg-Si compound particles on the surface of the coating. In order to achieve this purpose, the annealing temperature cannot be too low and the time cannot be too short. Too low temperature and too short time cannot play the effect of promoting the diffusion of Al and Mg outward, and cannot form enough Mg-Si compound particles. At the same time, the annealing temperature cannot be too high and the time cannot be too long, otherwise the oxide film will grow too thick and the size of the Mg-Si compound particles will be too large. Therefore, the invention requires the annealing temperature to be between 120°C and 320°C. The annealing time is 10 seconds to 60 seconds.

[0067] In addition, in the annealing process, the annealing atmosphere is also very important. In order to obtain the required oxide film on the coating surface, a certain amount of oxygen molecules is required in the annealing atmosphere, and the present invention requires 10%. However, if there are too many oxygen molecules, the surface oxide film will be too thick.

[0068] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then proceed according to general international standards, conventional conditions, or according to the conditions recommended by the manufacturer.

[0069] Examples 1-7 and Comparative Examples 1-5 provide a zinc-aluminum-magnesium coated steel sheet. The preparation method of the zinc-aluminum-magnesium coated steel sheet in each example is as follows: Figure 1 As shown, including:

[0070] Obtaining a steel plate substrate to be coated with a zinc-aluminum-magnesium coating;

[0071] The steel plate substrate is hot-dip plated, then annealed, cooled, skin-passed and coiled to obtain a zinc-aluminum-magnesium coated steel plate;

[0072] Wherein, the hot dip plating solution comprises the following components by mass fraction:

[0073] Al: 1-8%; Mg: 1-4%; Si: 0.001-0.1%; the rest is Zn and unavoidable impurities;

[0074] The annealing process parameters include: a temperature of 120° C. to 320° C., a time of 10s to 60s, and a molar fraction of oxygen molecules in the annealing atmosphere of 10% to 50%.

[0075] The specific parameters of the zinc-aluminum-magnesium coating in the zinc-aluminum-magnesium coated steel sheets provided in Examples 1-7 and Comparative Examples 1-5 are shown in Table 1, and the specific preparation process parameters of each example are shown in Table 2.

[0076] Table 1 Specific parameters of zinc-aluminum-magnesium coating in each case

[0077]

[0078]

[0079] Table 2 Specific preparation process parameters for each example

[0080]

[0081] Test Case

[0082] This example provides a zinc-aluminum-magnesium coated steel plate for example 1-7 and comparative example 1-5 to evaluate the surface friction coefficient and corrosion resistance. The test results are shown in Table 3.

[0083] The evaluation method is as follows: (1) fix the zinc-aluminum-magnesium coated steel plate on a horizontal base; (2) place a hard steel ball with a diameter of 6 mm in contact with the surface of the steel plate; (3) apply a vertical load of 500g on the surface of the steel ball so that the steel ball and the steel plate are pressed tightly; (4) apply a horizontal speed of 100mm / min and a distance of 10mm to the steel plate base so that friction occurs between the steel ball and the coating; (5) measure the horizontal friction force on the steel ball; (6) divide the friction force by the vertical load to obtain the friction coefficient; (7) repeat the measurement 5 times and take the average value. The corrosion resistance of the coating was evaluated by the neutral salt spray corrosion test. The zinc-aluminum-magnesium coated sample was placed in a neutral salt spray test environment for 500 hours. The sample size was 100mm×150mm and the coating thickness was 7 microns. The area ratio (%) of red rust on the coating surface was calculated. The neutral salt spray test method meets GB / T 10125.

[0084] Table 3 Test results of each case

[0085] serial number Average friction factor Red rust area ratio (%) Example 1 0.004 0.0% Example 2 0.005 0.0% Example 3 0.004 0.0% Example 4 0.003 0.0% Example 5 0.004 0.0% Example 6 0.005 0.0% Example 7 0.003 0.0% Comparative Example 1 0.009 12.0% Comparative Example 2 0.012 20.0% Comparative Example 3 0.013 0.0% Comparative Example 4 0.008 5.0% Comparative Example 5 0.011 3.0%

[0086] The microstructure of the zinc-aluminum-magnesium coating in the zinc-aluminum-magnesium coating steel sheet obtained in Example 1 is shown in FIG. Figure 2 As shown, the size of Mg-Si compound particles in the zinc-aluminum-magnesium coating is ≤5um.

[0087] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "include..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0088] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A zinc-aluminum-magnesium coating, characterized in that: The zinc-aluminum-magnesium coating comprises the following components: Al, Mg, Si, Zn and impurities from preparing the zinc-aluminum-magnesium coating; The surface of the zinc-aluminum-magnesium coating contains no less than 0.01% of Mg-Si compound particles by volume fraction, and the size of the Mg-Si compound particles is ≤5um, and the Mg-Si compound is an intermetallic compound Mg2Si formed by Mg and Si; The surface of the zinc-aluminum-magnesium coating contains an oxide layer with a thickness of 1-50 nm; The oxide includes at least one of an oxide of Al, an oxide of Mg and an oxide of Zn; In terms of mass fraction, the Mg element in the oxide is ≥ 10%, and / or the Al element in the oxide is ≥ 10%; The preparation method of the zinc-aluminum-magnesium coating comprises: hot-dip plating a steel plate substrate, followed by annealing, wherein the annealing process parameters include: a temperature of 120° C. to 320° C., a time of 10s to 60s, and a molar fraction of oxygen molecules in the annealing atmosphere of 10% to 50%; The zinc-aluminum-magnesium coating comprises the following components: Al: 1-8%; Mg: 1-4%; Si: 0.001-0.1%; the rest is Zn and impurities from preparing the zinc-aluminum-magnesium coating.

2. The zinc-aluminum-magnesium coating according to claim 1, characterized in that: Calculated by mass fraction, the Si element content in the zinc-aluminum-magnesium coated steel plate coating does not exceed one twentieth of the Mg element content.

3. The zinc-aluminum-magnesium coating according to any one of claims 1 to 2, characterized in that: The surface friction coefficient of the zinc-aluminum-magnesium coating is ≤0.

005.

4. A zinc-aluminum-magnesium coated steel sheet, characterized in that: The zinc-aluminum-magnesium coated steel plate comprises a steel plate substrate and a coating attached to the surface of the steel plate substrate; The coating is the zinc-aluminum-magnesium coating according to any one of claims 1 to 3.

5. A method for preparing the zinc-aluminum-magnesium coated steel sheet according to claim 4, characterized in that: The preparation method comprises: Obtaining a steel plate substrate to be coated with a zinc-aluminum-magnesium coating; The steel plate substrate is hot-dip plated, then annealed, cooled, skin-passed and coiled to obtain a zinc-aluminum-magnesium coated steel plate; Wherein, the hot dip plating solution comprises the following components by mass fraction: Al: 1-8%; Mg: 1-4%; Si: 0.001-0.1%; the rest is Zn and inevitable impurities.

Citation Information

Patent Citations

  • Method for plating surface of steel with Al-Zn-Mg-Si alloy plating layer in continuous hot-dipping manner

    CN105483594A

  • Aluminum-based alloy plated steel sheet having excellent processing part corrosion resistance

    CN110100039A

  • Microcrack-free hot-dip galvanized coated steel plate and preparation method thereof

    CN114369782A

  • Hot dip zn-al-mg-si plated steel excellent in corrosion resistance of uncoated part and coated edge face part

    JP2001355055A

  • Surface-treated hot-dip plated steel

    JP2013044024A

Cited By

  • Zinc-aluminum-magnesium composite steel plate for automobile and processing technology thereof

    CN122076843A