A preparation method of basic copper phosphate, a laser engraving material and its preparation method and application
By preparing alkaline copper phosphate with a particle size of less than 10μm and dispersing it evenly with the resin matrix, the problem of excessive particle size of commercial products is solved, the laser engraving effect in laser direct molding technology is improved, and the high laser engraving material is achieved Adhesion and good mechanical properties.
Patent Information
- Application Number
- CN202210758766.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-06-29
AI Technical Summary
The average particle size of commercially available basic copper phosphate is greater than 10 μm, resulting in poor dispersion and insufficient binding in laser direct molding technology, affecting the laser engraving effect.
By mixing and reacting alkaline copper carbonate and phosphoric acid, heating to boiling point, the liquid phase is separated, the average particle size of the obtained alkaline copper phosphate is less than 10 μm, and it is uniformly dispersed with the resin matrix and other filler or additive components, using machinery Stirring and specific process processing to improve metal adhesion.
It realizes a good combination of alkaline copper phosphate and resin matrix, improves the metal adhesion performance of laser activated components, improves the laser engraving effect, and provides high surface finish, fluidity and thin-wall toughness for radial engraving materials, suitable for LDS antenna housing or electronic housing products.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of laser forming, and in particular to a method for preparing basic copper phosphate, a laser engraving material, and a preparation method and application thereof. Background Art
[0002] Laser Direct Structuring (LDS) is a process currently widely used in many fields in developed countries. It was first invented by the German LPKF company and is a three-dimensional molded interconnect device production technology that integrates injection molding, laser processing and electroless chemical plating processes. It gives ordinary plastic components or circuit boards electrical interconnection functions, or enables plastic products to achieve electronic protection, physical mechanical and other functions, so as to achieve a high degree of integration between entities and conductive graphics and form 3D-MID, which can be applied to communications, automobiles, computers, electromechanical equipment, medical equipment and other industries.
[0003] The key to LDS is to add an exogenous additive that is sensitive to lasers, namely, laser engraving additives, to the plastic matrix; under the action of the laser, the structure of the laser engraving additive is destroyed, the ions are reduced to atoms and aggregated to form metal particles, which adhere to the resin surface ablated by the laser to form a metal core, and the metal core is used to achieve many functions in subsequent electroless chemical plating. The metal compounds in the laser engraving additive must be evenly distributed in the matrix, stably reduced to atoms after laser irradiation, and have high temperature resistance, insulation and other characteristics. Conventional laser engraving additives use copper as the metal element. It has been found that basic copper phosphate is a laser engraving raw material with good LDS performance, which can replace the original Cu-Cr spinel for laser direct forming technology; however, the average particle size of commercially available basic copper phosphate is usually greater than 10μm, which will lead to poor dispersion of laser-sensitive materials during laser activation processing and poor bonding with the resin substrate.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The first purpose of the present invention is to provide a method for preparing basic copper phosphate. The basic copper phosphate prepared by the preparation method overcomes the defect that the particle size of existing commercial products is too large. The basic copper phosphate prepared by the present invention has an average particle size of less than 10 μm. When used as a laser activated material in laser direct forming technology, it can be evenly dispersed and combined with a resin matrix and other filling or auxiliary components in the laser engraving material, thereby improving the metal adhesion of the laser activated component and ultimately achieving an improved laser engraving effect.
[0006] The second object of the present invention is to provide a laser engraving material which, when applied to LDS antenna housings or electronic housing products, has good surface finish, fluidity and thin-wall toughness.
[0007] The third object of the present invention is to provide a method for preparing the laser engraving material.
[0008] The fourth object of the present invention is to provide basic copper phosphate prepared by the preparation method of basic copper phosphate, and the use of the laser carving material in laser carving or laser activation.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] A method for preparing basic copper phosphate comprises the following steps: mixing basic copper carbonate and phosphoric acid for reaction, heating to boiling point, and then separating the liquid phase to obtain the basic copper phosphate;
[0011] Wherein, the bulk density of the basic copper carbonate is 100 g / L to 800 g / L; and the temperature of the mixing reaction is less than 70°C.
[0012] Preferably, the mixing comprises mechanical stirring;
[0013] More preferably, the frequency of the mechanical stirring is 100 rpm to 1000 rpm; the time of the mechanical stirring is 10 min to 100 min.
[0014] Preferably, the molar ratio of the basic copper carbonate to the phosphoric acid is 2:1 to 1.3;
[0015] More preferably, in the mixed solution of the basic copper carbonate and the phosphoric acid, when no reaction is performed, the mass concentration of the basic copper carbonate is 5% to 25%;
[0016] More preferably, the phosphoric acid is selected in a mass fraction of 65% to 85%.
[0017] A laser engraving material, comprising the following components by mass: 10 to 30 parts of basic copper phosphate prepared by the preparation method of basic copper phosphate as claimed in claims 1 to 3, 50 to 110 parts of a resin matrix, 0 to 30 parts of a filler and 0 to 10 parts of an additive;
[0018] Wherein, the resin matrix includes at least one of polyethylene, polypropylene, polycarbonate, polyurethane, petroleum resin, polybutylene terephthalate, polyamide or acrylonitrile-butadiene-styrene copolymer.
[0019] Preferably, the filler includes at least one of titanium dioxide, mica powder, silicon ball material, graphite, graphene or carbon fiber;
[0020] Preferably, the auxiliary agent includes at least one of a flame retardant, a coupling agent, a lubricant, an antioxidant, an anti-ultraviolet agent, a nucleating agent or a toughening agent.
[0021] Preferably, the composition comprises the following components by mass: 15 to 25 parts of basic copper phosphate prepared by the preparation method of basic copper phosphate, 80 to 100 parts of resin matrix, 10 to 20 parts of filler and 1 to 6 parts of auxiliary agent.
[0022] The preparation method of the laser engraving material comprises the following steps which are performed in sequence: a batching step, a grinding step, a mixing step, a drying step and a crushing step.
[0023] Preferably, the mixing process is carried out using a mixer or an extruder;
[0024] In the mixing process, the stirring and / or extrusion temperature is 250° C. to 300° C.; the stirring frequency is 300 rpm to 800 rpm, and / or the screw speed is 50 rpm to 250 rpm.
[0025] The basic copper phosphate prepared by the preparation method of basic copper phosphate and the laser carving material are used in laser carving or laser activation.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] (1) The average particle size of the basic copper phosphate prepared by the present invention is less than 10 μm; when it is used as a laser-sensitive component and applied in the field of laser forming, it has better adhesion performance when combined with a resin matrix with an equal amount of viscous components, and effectively prevents the metal coating from falling off, curling or hardening during the laser activation process.
[0028] (2) The laser material prepared by the present invention appears gray, gray-green or gray-black depending on the selection of the resin substrate or the filler, and has good surface properties and mechanical strength.
[0029] (3) The laser material prepared by the present invention has high surface finish, high fluidity and high thin-wall toughness, and can be used for LDS antenna housing or electronic housing products. DETAILED DESCRIPTION
[0030] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0031] The present invention is implemented by the following technical solutions:
[0032] A method for preparing basic copper phosphate comprises the following steps: mixing basic copper carbonate and phosphoric acid for reaction, heating to boiling point, and then separating the liquid phase to obtain the basic copper phosphate; wherein the bulk density of the basic copper carbonate is 100 g / L to 800 g / L; and the temperature of the mixing reaction is less than 70°C.
[0033] In actual production, common basic copper carbonate can be purchased through commercial channels, and its real density, bulk density, particle size, volume, mass and other specification parameters are measured. Then, at least one of crushing, rolling, grinding, ultrasound and vibration is used to select a method based on the original specification parameters and the density parameters actually required, and a basic copper carbonate raw material with a bulk density of 100 g / L to 800 g / L is obtained through conventional parameter setting.
[0034] It should be noted that all bulk densities involved in the present invention are tested and implemented in accordance with German industrial standard DIN 53,468.
[0035] As a preferred embodiment, the bulk density of the basic copper carbonate is 200g / L to 600g / L; the bulk density of the basic copper carbonate includes but is not limited to 200g / L, 250g / L, 300g / L, 350g / L, 400g / L, 450g / L, 500g / L, 550g / L, and 600g / L.
[0036] As a preferred embodiment, the temperature of the mixed reaction includes but is not limited to 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, and 60°C.
[0037] As a preferred embodiment, the mixing includes mechanical stirring; the frequency of the mechanical stirring includes but is not limited to 100rpm, 150rpm, 200rpm, 250rpm, 300rpm, 350rpm, 400rpm, 450rpm, 500rpm, 550rpm, 600rpm, 650rpm, 700rpm, 750rpm, 800rpm, 850rpm, 900rpm, 950rpm, 1000rpm; the time of the mechanical stirring includes but is not limited to 10min, 20min, 30min, 40min, 50min, 60min, 70min, 80min, 90min, 100min.
[0038] As a preferred embodiment, the dosage of the phosphoric acid is at least the dosage for theoretical complete reaction, or the dosage of the phosphoric acid is 5% to 10% higher than the dosage for theoretical complete reaction; the molar ratio of the basic copper carbonate to the phosphoric acid includes but is not limited to 2:1, 2:1.1, 2:1.2, and 2:1.3.
[0039] As a more preferred embodiment, in the mixed solution of the basic copper carbonate and the phosphoric acid, when no reaction is carried out, the mass concentration of the basic copper carbonate includes but is not limited to 5%, 10%, 15%, 20%, 25%; the mass fraction of the phosphoric acid includes but is not limited to 65%, 70%, 75%, 80%, 85%.
[0040] A laser engraving material comprises the following components by mass: 10 to 30 parts of basic copper phosphate prepared by the preparation method of basic copper phosphate as described above, 50 to 110 parts of a resin matrix, 0 to 30 parts of a filler and 0 to 10 parts of an additive;
[0041] Wherein, the resin matrix includes at least one of polyethylene (PE), polypropylene (PP), polycarbonate (PC), polyurethane (PU), hydrocarbon resin, polybutylene terephthalate (PBT), polyamide (PA) or acrylonitrile-butadiene-styrene copolymer (ABS).
[0042] As a preferred embodiment, the filler includes at least one of titanium dioxide, mica powder, silicon ball material, graphite, graphene or carbon fiber; the auxiliary agent includes at least one of flame retardant, coupling agent, lubricant, antioxidant, anti-ultraviolet agent, nucleating agent or toughening agent.
[0043] For the resin matrix, the filler and the auxiliary agent, any one, any two or a combination of any several of those mentioned in the present invention may be selected; the present invention does not limit the specific type selection and quantity.
[0044] As a preferred embodiment, the weight parts of basic copper phosphate include but are not limited to 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, and 25 parts, the weight parts of the resin matrix include but are not limited to 80 parts, 81 parts, 82 parts, 83 parts, 84 parts, 85 parts, 86 parts, 87 parts, 88 parts, 89 parts, 90 parts, 91 parts, 92 parts, 93 parts, 94 parts, 95 parts, 96 parts, 97 parts, 98 parts, 99 parts, and 100 parts, the weight parts of the filler include but are not limited to 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, and 20 parts, and the weight parts of the additives include but are not limited to 1 part, 2 parts, 3 parts, 4 parts, 5 parts, and 6 parts.
[0045] The preparation method of the laser engraving material comprises the following steps which are performed in sequence: a batching step, a grinding step, a mixing step, a drying step and a crushing step.
[0046] Among them, the batching process is used to weigh the required mass fractions of raw materials, the grinding process is used to process the raw materials to meet the specification parameters of the feed, the mixing process is used to evenly disperse the raw materials under specific temperature, pressure, and frequency conditions to make them into uniform mixed components, as well as necessary post-processing steps such as the drying process and the crushing process.
[0047] As a preferred embodiment, the mixing process is carried out using a mixer or an extruder; wherein the temperature of the mixing process includes but is not limited to 250°C, 260°C, 270°C, 280°C, 290°C, and 300°C; when a mixer is used for the mixing, the stirring frequency includes but is not limited to 300rpm, 400rpm, 500rpm, 600rpm, 700rpm, and 800rpm; when an extruder is used for the mixing, the screw speed includes but is not limited to 50rpm, 100rpm, 150rpm, 200rpm, and 250rpm.
[0048] The basic copper phosphate prepared by the preparation method of basic copper phosphate and the laser carving material are used in laser carving or laser activation.
[0049] Example 1
[0050] (1) Preparation of basic copper phosphate: 2 liters of deionized water, 200 grams of basic copper carbonate (bulk density 200 g / L after vibration treatment) and 200 grams of 85% phosphoric acid are placed in a container for sufficient reaction, a constant temperature water bath of 50° C. and a stirrer at 550 rpm are set; after reacting for 20 minutes, the reaction liquid is heated to boiling; after maintaining the boiling state for 10 minutes, the reaction liquid is filtered to separate the liquid phase, and low-temperature drying is performed to obtain basic copper phosphate.
[0051] (2) Raw material components: 60 parts of polycarbonate, 30 parts of acrylonitrile-butadiene-styrene copolymer, 20 parts of basic copper phosphate, 15 parts of carbon fiber, 0.5 parts of antioxidant, 0.5 parts of lubricant, and 1 part of flame retardant.
[0052] (3) Preparation process: A mixer is used for stirring and then drying. The specific parameter settings are shown in Table 1 below;
[0053] Table 1 Parameter settings
[0054]
[0055] (4) Performance effect:
[0056] Table 2 Result parameter table
[0057]
[0058]
[0059] Example 2
[0060] (1) Preparation of basic copper phosphate: the same as in Example 1.
[0061] (2) Raw material components: 40 parts of polypropylene, 30 parts of C9 petroleum resin, 20 parts of nylon PA66, 20 parts of basic copper phosphate, 15 parts of titanium dioxide, 0.5 parts of antioxidant, 1.5 parts of lubricant, and 1 part of flame retardant.
[0062] (3) Preparation process: A mixer is used for stirring and then drying. The specific parameter settings are shown in Table 3 below;
[0063] Table 3 Parameter settings
[0064]
[0065] (4) Performance effect:
[0066] Table 4 Result parameter table
[0067]
[0068]
[0069] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A laser engraving material, characterized in that: The invention is composed of the following components by mass: 10 to 30 parts of basic copper phosphate, 50 to 110 parts of a resin matrix, 10 to 20 parts of a filler and 1 to 6 parts of an additive; Wherein, the resin matrix includes at least one of polyethylene, polypropylene, polycarbonate, polyurethane, petroleum resin, polybutylene terephthalate, polyamide or acrylonitrile-butadiene-styrene copolymer; the filler includes one of carbon fiber or titanium dioxide; the additive includes flame retardant, lubricant and antioxidant; The preparation method of basic copper phosphate comprises the following steps: mixing basic copper carbonate and phosphoric acid for reaction, heating to boiling point, and then separating the liquid phase to obtain the basic copper phosphate; wherein the bulk density of the basic copper carbonate is 100 g / L to 800 g / L; the temperature of the mixing reaction is less than 70° C.; and the average particle size of the basic copper phosphate is less than 10 μm.
2. The laser engraving material according to claim 1, characterized in that: The mixing includes mechanical stirring; The frequency of the mechanical stirring is 100 rpm to 1000 rpm; the time of the mechanical stirring is 10 min to 100 min.
3. The laser engraving material according to claim 1, characterized in that: The molar ratio of the basic copper carbonate to the phosphoric acid is 2:1 to 1.
3.
4. The laser engraving material according to claim 1, characterized in that: In the mixed solution of the basic copper carbonate and the phosphoric acid, when no reaction is performed, the mass concentration of the basic copper carbonate is 5% to 25%.
5. The laser engraving material according to claim 1, characterized in that: The phosphoric acid is selected in a mass fraction of 65% to 85%.
6. The laser engraving material according to claim 1, characterized in that: It includes the following components by mass: 15 to 25 parts of basic copper phosphate, 80 to 100 parts of resin matrix, 10 to 20 parts of filler and 1 to 6 parts of auxiliary agent.
7. The method for preparing the laser engraving material according to claim 1, characterized in that: The process includes the following steps: Batching process, grinding process, mixing process, drying process and crushing process.
8. The method for preparing laser engraving material according to claim 7, characterized in that: The mixing process is carried out using a mixer or an extruder; In the mixing process, the stirring and / or extrusion temperature is 250° C. to 300° C.; the stirring frequency is 300 rpm to 800 rpm, and / or the screw speed is 50 rpm to 250 rpm.
9. Use of the laser engraving material according to any one of claims 1 to 6 in laser engraving or laser activation.
Citation Information
Cited By
Dumbbell-shaped basic phosphate material as well as preparation method and application thereof
CN116675199A
A dumbbell-shaped basic phosphate material, a preparation method and application thereof