Preparation method of magnetic polydopamine-modified CuS nanoparticles with high solar energy absorption
CuS nanoparticles are prepared and modified by dopamine through hydrothermal method, combined with magnetic transition metal oxides, and solved the problems of low efficiency and poor recycling and utilization of existing solar photothermal conversion materials, and achieved efficient solar photothermal conversion and material recycling. Suitable for seawater desalination and other applications.
Patent Information
- Application Number
- CN202211376302.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-04
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-11-04
AI Technical Summary
The existing solar photothermal conversion materials have low photothermal conversion efficiency and lack good recycling and utilization, making it difficult to effectively utilize solar radiation energy.
Hydrothermal ultrasonic method was used to prepare CuS sheet-type matrix, and magnetic polydopamine-modified CuS nanoparticles were prepared by combining dopamine modification and magnetic transition metal oxides to enhance their photothermal absorption performance and realize material recovery through magnetic properties. use.
It significantly improves the photothermal conversion efficiency of solar energy, can absorb it in a wide range of solar spectrum, and achieves efficient recycling and reuse of materials through magnetic separation, and is suitable for fields such as seawater desalination.
Smart Images

Figure CN115611347B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing magnetic polydopamine-modified CuS nanoparticles with high solar energy absorption, and belongs to the technical field of preparation of solar energy photothermal conversion absorption materials. Background Art
[0002] As people's awareness of environmental protection and energy conservation and emission reduction increases, the search for the use of renewable energy has attracted people's attention. Among all renewable energy sources, solar energy is one of the most promising energy sources. In recent years, many studies have focused on solar energy utilization technology.
[0003] At present, the development of solar energy utilization technology in the world is mainly concentrated in two major areas, namely photovoltaic conversion and photothermal conversion. However, photovoltaic conversion can only occur within a narrow spectrum range, and the industry's high-level photoelectric conversion efficiency is difficult to exceed 27%. In contrast, solar photothermal conversion technology can not only utilize more than 99% of solar radiation energy, but also achieve a solar energy conversion efficiency of more than 90%.
[0004] Solar thermal conversion materials mainly inherit the inherent characteristics of absorbers to convert energy. Commonly used intrinsic absorption materials are mainly composed of semiconductors and oxides, nitrides, and sulfides of transition metals. They are characterized by a large number of orbits that can be used to absorb photon energy. According to band theory analysis, when the photon energy is greater than the bandgap width of the intrinsic absorption material, photons of sufficient energy will cause electron excitation and transition from the valence band to the empty conduction band. Free electrons will be generated in the conduction band, leaving holes in the valence band. In this process, the photon energy is absorbed and released in the form of heat energy. In addition, in addition to the above-mentioned photothermal conversion performance, some transition metal oxides also have excellent magnetic properties, which greatly enriches the application scenarios of the materials.
[0005] In recent years, new dopamine-based solar thermal conversion materials have been discovered and studied by inventors. Although the photothermal conversion efficiency of this emerging material is lower than that of traditional solar absorption materials, due to the superior adhesion of polydopamine and the large number of modifiable groups it carries, the field of dopamine-modified materials has flourished. Summary of the invention
[0006] The purpose of the present invention is to combine the advantages of the above materials and overcome their shortcomings, and provide a method for preparing magnetic polydopamine-modified CuS nanoparticles with high solar energy absorption prepared by combining the advantages of transition metal oxides, semiconductors and dopamine, which can improve the photothermal absorption performance of the material and have good recyclability.
[0007] The technical solution of the present invention is a method for preparing magnetic polydopamine-modified CuS nanoparticles with high solar energy absorption. First, a CuS sheet-type matrix is prepared by hydrothermal ultrasound, then CuS is added to a dopamine solution to form polydopamine-modified CuS nanoparticles, and finally a solvent method is used to in-situ grow a magnetic transition metal oxide on polydopamine to prepare CuS nanoparticles containing magnetic polydopamine modification.
[0008] Further, the steps are as follows:
[0009] (1) Preparation of sheet-like nano CuS: adding a measured amount of copper source and sulfur source to deionized water, stirring with a magnetic force, and adjusting the pH value of the solution with hydrochloric acid; heating and keeping the solution for a period of time, and after cooling to room temperature, removing the upper clear liquid, and washing the lower dark slurry with ethanol and deionized water; centrifuging several times for passivation, and calcining at high temperature to obtain CuS nanosheets;
[0010] (2) Preparation of dopamine-modified CuS nanosheets: The CuS prepared in step (1) is ultrasonically dispersed in a Tris buffer solution, and then dopamine hydrochloride is added and magnetically stirred at room temperature; after the reaction is completed, the product is washed several times with deionized water and dried to obtain a polydopamine-modified CuS nanosheet product;
[0011] (3) Preparation of magnetic polydopamine-modified CuS nanoparticles: The polydopamine-modified CuS nanosheets prepared in step (2) were ultrasonically dispersed in deionized water; a measured amount of Fe 2+ and Fe 3+ The precursor is continuously stirred, and then the pH value of the solution is adjusted to alkaline with aqueous ammonia; a dispersant is added and stirred vigorously; the black product is washed and dried to obtain magnetic polydopamine-modified CuS nanoparticles.
[0012] Furthermore, the copper source is specifically one or more of copper nitrate, copper chloride and copper sulfate.
[0013] Furthermore, the sulfur source is specifically thiourea.
[0014] Further, the iron ion precursor is specifically one or more of ferric chloride, ferric nitrate and ferric sulfate;
[0015] Furthermore, the ferrous ion precursor is specifically one or more of ferrous sulfate, ferrous chloride and ferrous carbonate.
[0016] Further, step (1) is as follows: deionized water is boiled for deoxygenation treatment and then set aside; 0.4-0.5g of copper salt, 1.5-1.6g of sulfur source and 70mL of deionized water are added to a reaction container in sequence, and magnetically stirred at 200-400rpm to be uniform, and after the solution is uniformly mixed, hydrochloric acid is added to adjust the pH to 1, and then stirring is continued for 40min; the uniformly mixed solution is transferred to a polytetrafluoroethylene hydrothermal synthesis kettle, sealed and then transferred to a programmable box furnace, and kept warm at 175-185°C for 18-22h; after cooling to room temperature, the upper clear liquid is poured off, the lower black slurry is washed with ethanol and deionized water, purified by centrifugation at a speed of 7000-9000rmp for 8-12min, dried and ground in a vacuum oven at 55-65°C and 0.08-0.1MPa, and then transferred to a programmable box furnace, and kept warm at 275- The powder was calcined at 285°C for 2-4 hours, and the calcined powder was further ground and passed through a 200-mesh sieve to obtain CuS nanosheets.
[0017] Furthermore, step (2) is: 1.2-1.3g Tris and 90-100mg CuS nanosheets prepared in step (1) are ultrasonically dispersed in a flask at a power of 140-160W, and magnetically stirred at 200-400rpm for 10-20min, and then 140-150mg dopamine hydrochloride is added, and the reaction is carried out at a speed of 50-100rpm at room temperature for 3-5h; after the reaction is completed, the obtained black insoluble matter is washed with deionized water, and finally vacuum dried at 55-65°C and 0.08-0.1MPa to obtain polydopamine-modified CuS nanosheets.
[0018] Further, step (3) is: 90-100 mg of the polydopamine-modified CuS nanosheets prepared in step (2) and 180-220 mL of deionized water are added to a reaction container, and ultrasonically dispersed at 140-160 W for 4-6 min at room temperature. Then, 20-25 mmol of Fe 3+ Precursor and 10-12.5 mol Fe 2+ Precursor, the solution is stirred at 200-400 rpm for 1 hour; then 15-25 mL 25 wt% ammonia solution and 6-7 g citric acid are added to the above solution and reacted for 1 hour; finally, the black precipitate is separated by a magnet and washed and dried to obtain magnetic polydopamine modified CuS nanoparticles.
[0019] The magnetic polydopamine-modified CuS nanoparticles prepared by the method are applied in the field of seawater distillation and desalination.
[0020] From the composition point of view, whether it is CuS, Fe3O4 or polydopamine, the magnetic dopamine-modified CuS nanomaterials are commonly used materials in the field of solar thermal energy, and different materials have different bandgap widths. The magnetic polydopamine-modified CuS can exert the synergistic effect of materials and absorb in a wide range of the solar spectrum. In terms of structure, the lamellar CuS material can greatly increase the area receiving light, and the polydopamine particles on the flaky material can increase the probability of multi-level reflection and scattering of light, which increases the absorption efficiency. In terms of application, the magnetic Fe3O4 allows the material to be separated using a magnet, which allows the material to be recycled and reused after desalination of seawater.
[0021] Beneficial effects of the present invention: The method of the present invention can prepare high-performance solar thermal conversion materials. The material can utilize solar energy to the maximum extent to produce photothermal effects and can be widely used in seawater desalination or other solar thermal collection fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 At 1.0kw / m 2 Schematic diagram of the evaporation amount of water-time of the magnetic polydopamine-modified CuS prepared in Example 1 of the present invention under simulated sunlight conditions and without the addition of modified CuS.
[0023] Figure 2 Schematic diagram of the magnetic experimental results of magnetic polydopamine modified CuS nanoparticles.
[0024] Figure 3 It is the reflectance spectra of CuS and magnetic polydopamine-modified CuS. DETAILED DESCRIPTION
[0025] Example 1
[0026] (1) Preparation of sheet-like nano CuS: Deionized water was boiled and deoxygenated for later use; 0.47g Cu(NO3)2, 1.52g H2NSCNH2 and 70mL deionized water were added to the reaction vessel in sequence, and magnetic stirring was performed at 300rpm to mix the solution evenly. After the solution was mixed evenly, hydrochloric acid was added to adjust the pH to 1, and then stirring was continued for 40min. The mixed solution was transferred to a polytetrafluoroethylene hydrothermal synthesis reactor, sealed and transferred to a programmable box furnace, and kept at 180℃ for 20h. After cooling to room temperature, the upper clear liquid was poured off, and the lower black slurry was washed with ethanol and deionized water, centrifuged at 8000rmp for 10min for purification, dried and ground in a 60℃ vacuum oven, and then transferred to a programmable box furnace, calcined at 280℃ for 3h, and the calcined powder was further ground and passed through a 200-mesh sieve to obtain CuS nanosheets.
[0027] (2) Preparation of dopamine-modified CuS nanosheets: 1.25 g Tris and 100 mg CuS nanosheets prepared in step (1) were ultrasonically dispersed in a flask at 150 W power, and magnetically stirred at 200-400 rpm for 15 min, and then 150 mg dopamine hydrochloride was added and reacted at 50-100 rpm for 4 h at room temperature. After the reaction, the obtained black insoluble matter was washed with deionized water, and finally vacuum dried at 60° C. and 0.08 MPa to obtain polydopamine-modified CuS nanosheets.
[0028] (3) Preparation of magnetic dopamine-modified CuS nanosheets: 100 mg of the polydopamine-modified CuS nanosheets prepared in step (2) and 200 mL of deionized water were added to a reaction vessel and ultrasonically dispersed at 150 W for 5 min at room temperature. Then, 22 mmol of FeCl3·6H2O and 11 mmol of FeSO4·7H2O were added to the above solution, and the solution was stirred at 300 rpm for 1 h. Then, 20 mL of 25 wt% ammonia solution and 6 g of citric acid were added to the above solution and reacted for 1 h. Finally, the black precipitate was separated by a magnet and washed and dried to obtain magnetic polydopamine-modified CuS nanoparticles.
[0029] Example 2
[0030] (1) Preparation of sheet-like nano CuS: Deionized water was boiled and deoxygenated for later use; 0.4 g of copper salt, 1.5 g of sulfur source and 70 mL of deionized water were added to a reaction vessel in sequence, and magnetically stirred at 200 rpm. After the solution was mixed evenly, hydrochloric acid was added to adjust the pH to 1, and then stirring was continued for 40 min; the mixed solution was transferred to a polytetrafluoroethylene hydrothermal synthesis reactor, sealed, and then transferred to a programmable box furnace and kept at 175°C for 22 h; after cooling to room temperature, the upper clear liquid was poured off, and the lower black slurry was washed with ethanol and deionized water, purified by centrifugation at 7000 rpm for 12 min, dried and ground in a vacuum oven at 55°C and 0.08 MPa, and then transferred to a programmable box furnace and calcined at 275°C for 4 h. The calcined powder was further ground and passed through a 200-mesh sieve to obtain CuS nanosheets.
[0031] (2) Preparation of dopamine-modified CuS nanosheets: 1.2 g Tris and 90 mg CuS nanosheets prepared in step (1) were ultrasonically dispersed in a flask at 140 W power, and magnetically stirred at 200 rpm for 10 min. Then, 140 mg dopamine hydrochloride was added and reacted at 50 rpm for 5 h at room temperature. After the reaction, the obtained black insoluble matter was washed with deionized water, and finally vacuum dried at 55° C. and 0.08 MPa to obtain polydopamine-modified CuS nanosheets.
[0032] (3) Preparation of magnetic polydopamine-modified CuS nanoparticles: 90 mg of the polydopamine-modified CuS nanosheets prepared in step (2) and 180 mL of deionized water were added to a reaction vessel and ultrasonically dispersed at 140 W for 6 min at room temperature. Then, 20 mmol of Fe 3+ Precursor and 10 mol Fe 2+ Precursor, the solution was stirred at 200 rpm for 1 hour; then 15 mL of 25 wt% ammonia solution and 6 g of citric acid were added to the above solution and reacted for 1 hour; finally, the black precipitate was separated by a magnet and washed and dried to obtain magnetic polydopamine-modified CuS nanoparticles.
[0033] The copper source is specifically copper nitrate.
[0034] The sulfur source is specifically thiourea.
[0035] The iron ion precursor is specifically ferric chloride; the ferrous ion precursor is specifically ferrous sulfate.
[0036] Example 3
[0037] (1) Preparation of sheet-like nano CuS: Deionized water was boiled and deoxygenated for later use; 0.5 g of copper salt, 1.6 g of sulfur source and 70 mL of deionized water were added to a reaction vessel in sequence, and magnetically stirred at 400 rpm. After the solution was mixed evenly, hydrochloric acid was added to adjust the pH to 1, and then stirring was continued for 40 min; the mixed solution was transferred to a polytetrafluoroethylene hydrothermal synthesis reactor, sealed, and then transferred to a programmable box furnace and kept at 185°C for 18 h; after cooling to room temperature, the upper clear liquid was poured off, and the lower black slurry was washed with ethanol and deionized water, purified by centrifugation at 9000 rpm for 8 min, dried and ground in a 65°C, 0.1 MPa vacuum oven, and then transferred to a programmable box furnace and calcined at 285°C for 2 h. The calcined powder was further ground and passed through a 200-mesh sieve to obtain CuS nanosheets.
[0038] (2) Preparation of dopamine-modified CuS nanosheets: 1.3 g Tris and 100 mg CuS nanosheets prepared in step (1) were ultrasonically dispersed in a flask at 160 W power, and magnetically stirred at 200 rpm for 20 min. Then, 150 mg dopamine hydrochloride was added and reacted at 100 rpm for 3 h at room temperature. After the reaction, the obtained black insoluble matter was washed with deionized water, and finally dried in a vacuum at 65° C. and 0.1 MPa to obtain polydopamine-modified CuS nanosheets.
[0039] (3) Preparation of magnetic polydopamine-modified CuS nanoparticles: 100 mg of the polydopamine-modified CuS nanosheets prepared in step (2) and 220 mL of deionized water were added to a reaction vessel and ultrasonically dispersed at 160 W for 4 min at room temperature. Then, 25 mmol of Fe 3+ Precursor and 12.5 mol Fe 2+ Precursor, the solution was stirred at 400 rpm for 1 hour; then 25 mL of 25 wt% ammonia solution and 7 g of citric acid were added to the above solution and reacted for 1 hour; finally, the black precipitate was separated by a magnet and washed and dried to obtain magnetic polydopamine-modified CuS nanoparticles.
[0040] The copper source is specifically copper sulfate.
[0041] The sulfur source is specifically thiourea.
[0042] The iron ion precursor is specifically ferric nitrate; the ferrous ion precursor is specifically ferrous chloride.
[0043] Application Example 1
[0044] At 1.0kw / m 2 The amount of water evaporated by the magnetic polydopamine-modified CuS prepared in Example 1 of the present invention and without modified CuS under simulated sunlight conditions. The experimental process is as follows: 1g of modified CuS nanosheets and 1g of unmodified CuS nanosheets are placed in beakers containing 500mL of water, respectively, and a beaker containing 500mL of water without addition is used as a blank group. The three groups of samples are placed on a balance under simulated sunlight conditions and the weight is recorded once a minute. The graph is plotted with time as the horizontal axis and the evaporated weight as the vertical axis.
[0045] The experimental results are as follows Figure 1 As shown. Figure 1 It can be seen that the addition of nanopowder particles significantly improves the evaporation effect of water. The optimized and modified magnetic dopamine-modified CuS nanosheets can further improve the evaporation efficiency of water, and the effect becomes more significant as time goes by.
[0046] Application Example 2
[0047] The magnetic dopamine-modified CuS nanosheets prepared in Example 1 were tested for their magnetic properties. Figure 2 As shown. Figure 2 It can be seen that the modified CuS has excellent magnetic properties, which can greatly improve the recyclability of the powder.
[0048] Application Example 3
[0049] The magnetic dopamine-modified CuS nanosheets and ordinary CuS prepared in Example 1 were used to test their solar energy absorptivity. The calculation formula of the solar energy absorptivity α is as follows:
[0050]
[0051] Where G(λ) is the solar radiation intensity at air mass AM1.5, and ρ(λ) is the reflectivity of the powder, which can be measured by a standard UV-VIS-NIR spectrophotometer.
[0052] Specific test results such as Figure 3 As shown, the results indicate that the magnetic dopamine-modified CuS nanosheets have a high absorptivity of 96% within the 300-2000nm solar spectrum.
Claims
1. A method for preparing magnetic polydopamine-modified CuS nanoparticles with high solar energy absorption, characterized in that: First, a CuS sheet matrix is prepared by hydrothermal ultrasound, then CuS is added to a dopamine solution to form polydopamine-modified CuS nanoparticles, and finally a magnetic transition metal oxide is grown in situ on polydopamine by a solvent method to prepare CuS nanoparticles containing magnetic polydopamine modification; the specific steps are as follows: (1) Preparation of sheet-like nano CuS: Deionized water was boiled for deoxygenation and then set aside; 0.4-0.5 g of copper salt, 1.5-1.6 g of sulfur source and 70 mL of deionized water were added to a reaction vessel in sequence and magnetically stirred at 200-400 rpm. After the solution was mixed evenly, hydrochloric acid was added to adjust the pH to 1, and then stirring was continued for 40 min; the mixed solution was transferred to a polytetrafluoroethylene hydrothermal synthesis reactor, sealed and then transferred to a programmable box furnace and heated at 175 -185°C for 18-22h; after cooling to room temperature, pour off the upper clear liquid, wash the lower black slurry with ethanol and deionized water, purify by centrifugation at 7000-9000rpm for 8-12min, dry and grind in a vacuum oven at 55-65°C and 0.08-0.1MPa, transfer to a programmable box furnace, calcine at 275-285°C for 2-4h, further grind the calcined powder, and pass it through a 200-mesh sieve to obtain CuS nanosheets; (2) Preparation of dopamine-modified CuS nanosheets: 1.2-1.3 g Tris and 90-100 mg CuS nanosheets prepared in step (1) were ultrasonically dispersed in a flask at a power of 140-160 W, and magnetically stirred at 200-400 rpm for 10-20 min, then 140-150 mg dopamine hydrochloride was added, and the mixture was reacted at a speed of 50-100 rpm for 3-5 h at room temperature; after the reaction, the obtained black insoluble matter was washed with deionized water, and finally vacuum dried at 55-65° C. and 0.08-0.1 MPa to obtain polydopamine-modified CuS nanosheets; (3) Preparation of magnetic polydopamine-modified CuS nanoparticles: 90-100 mg of polydopamine-modified CuS nanosheets prepared in step (2) and 180-220 mL of deionized water were added to a reaction vessel and ultrasonically dispersed at 140-160 W for 4-6 min at room temperature. Then, 20-25 mmol of Fe 3+ Precursor and 10-12.5 mol Fe 2+ Precursor, the solution is stirred at 200-400 rpm for 1 hour; then 15-25 mL of 25 wt% ammonia solution and 6-7 g of citric acid are added to the above solution and reacted for 1 hour; finally, the black precipitate is separated by a magnet and washed and dried to obtain magnetic polydopamine-modified CuS nanoparticles.
2. The method for preparing the magnetic polydopamine-modified CuS nanoparticles with high solar absorption as claimed in claim 1, characterized in that: The copper salt is specifically one or more of copper nitrate, copper chloride and copper sulfate.
3. The method for preparing the magnetic polydopamine-modified CuS nanoparticles with high solar absorption as claimed in claim 1, characterized in that: The sulfur source is specifically thiourea.
4. The method for preparing the magnetic polydopamine-modified CuS nanoparticles with high solar absorption as claimed in claim 1, characterized in that: The iron ion precursor is specifically one or more of ferric chloride, ferric nitrate and ferric sulfate.
5. The method for preparing the magnetic polydopamine-modified CuS nanoparticles with high solar energy absorption as claimed in claim 4, characterized in that: The ferrous ion precursor is specifically one or more of ferrous sulfate, ferrous chloride and ferrous carbonate.
6. The magnetic polydopamine-modified CuS nanoparticles prepared by the method according to any one of claims 1 to 5, characterized in that: It is applied in the field of seawater distillation and desalination.