A high temperature resistant semi-aromatic copolyamide and its preparation method, composition and molded product
Semiar aromatic copolyamides with excellent mechanical properties and high thermal stability were prepared by using a specific combination of 1,10-decyldiamine and aromatic diacid in high temperature resistant polyamides, which solved the poor melt flowability of existing materials. and processing narrow window problems simplify the preparation process and meet the high heat resistance needs of the automotive industry.
Patent Information
- Application Number
- CN202110799801.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-07-15
AI Technical Summary
The existing high-temperature resistant polyamides have poor melt flowability and narrow melt processing windows, which are difficult to meet the high heat resistance and processing performance requirements of the automotive industry for materials, and the preparation process is complex.
A high-temperature resistant semi-aromatic copolyamide, whose monomer raw materials include 1,10-decyldiamine and aromatic diacid, are prepared by combining a specific molar ratio and additives, and a melting point above 270°C and a relative viscosity of 2.2 to 3.0. The copolyamide has a water absorption rate of 0.1 to 1%, and a simplified preparation method is adopted, including heating reaction, drainage concentration, exhaust pressure reduction and vacuum treatment.
The excellent mechanical properties, low water absorption and high thermal deformation temperature of copolyamide are achieved, the preparation process is simplified, quantitative production is facilitated, and the scope of use of polyamide is expanded.
Smart Images

Figure BDA0003164230440000091
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer materials, and in particular relates to a high temperature resistant low aromatic copolyamide and a preparation method and a composition thereof. Background Art
[0002] With the rise of surface mount technology (SMT) and the strong development trend of "plastic replacing steel" in the automotive industry, the market demand for high-temperature resistant polyamide has increased dramatically. SMT technology requires the melting point of the material to be no less than 215°C, and lead-free solder has put forward higher requirements for the heat resistance of the material. The increase in the combustion temperature of automobile fuel helps to fully burn the fuel, reduce fuel consumption, and reduce the emission of carbon dioxide and other toxic gases. The increase in the combustion temperature of fuel requires the peripheral parts of the automobile engine to have higher heat resistance. Traditional general-purpose plastics and ordinary engineering plastics can no longer meet the market demand for material heat resistance. The melting point of high-temperature resistant polyamide is higher than 270°C, and it has excellent short-term and long-term heat resistance. Common high-temperature resistant polyamides include PA46, PA5T, PA6T, PA9T, PA10T, PA11T, PA12T, PA MXD6, PMIA, PPTA, etc. PA10T, the full name of poly(decane terephthalamide), has high rigidity, high heat resistance, high mechanical strength and high dimensional stability due to the benzene ring structure of terephthalic acid. The long carbon chain structure of 1,10-decanediamine gives PA10T the advantages of melt processability and low water absorption. 1,10-decanediamine can be obtained from biomass raw material castor oil through saponification, cracking, amination and other steps. Therefore, PA10T is a bio-based high-temperature resistant polyamide with great development prospects. Similar to other semi-aromatic high-temperature resistant polyamides, PA10T has the disadvantages of poor melt fluidity and narrow melt processing window, so other comonomers are often introduced to improve its melt fluidity and reduce the melting point.
[0003] Patent CN101759853B provides a method for preparing semi-aromatic polyamide: first, monomers and additives are added to a polymerization kettle for condensation polymerization to obtain a prepolymer with a low intrinsic viscosity, and then the prepolymer is transferred to a viscosity increasing device for solid phase viscosity increasing after drying. However, this method uses a large number of equipment types and is complicated to operate. Summary of the invention
[0004] In order to solve the deficiencies of the prior art and products, the present invention provides a high temperature resistant semi-aromatic copolyamide and a preparation method, a composition and a molded product thereof.
[0005] The monomer raw materials of the copolyamide include diacid monomers and diamine monomers. The diacid monomers include but are not limited to aromatic dibasic acids and / or their derivatives, and aliphatic dibasic acids. The diamine monomers include but are not limited to decanediamine and pentamethylenediamine. The molar ratio of decanediamine to pentamethylenediamine is (1-30):1.
[0006] The 1,10-decanediamine (hereinafter referred to as decanediamine) is 1,10-decanediamine of chemical or biological origin, preferably 1,10-decanediamine of biological origin. The 1,5-pentanediamine (hereinafter referred to as pentamethylenediamine) in the monomer is pentamethylenediamine of chemical or biological origin, preferably 1,5-pentamethylenediamine of biological origin.
[0007] As an embodiment of the present invention, the molar ratio of decanediamine to aromatic dicarboxylic acid is 1:(0.7-1.5), further 1:(0.8-1.2), for example 1:0.98, 1:0.95.
[0008] As one embodiment of the present invention, the molar ratio of decanediamine to pentamethylenediamine is (2-40):1, further (2-30):1, further (2-20):1, for example, 19:1, 18:1, 10:1, 6.5:1, 4:1.
[0009] As an embodiment of the present invention, the molar ratio of the diamine monomer to the diacid monomer is (1-1.3):1, further (1-1.1):1, further (1-1.06):1, further (1.01-1.04):1.
[0010] As an embodiment of the present invention, the total amount of the diamine monomer and the diacid monomer accounts for more than 85%, further more than 90%, further more than 95%, further more than 97% of the total amount of monomer raw materials of the copolyamide, and the percentages are molar percentages.
[0011] As an embodiment of the present invention, the total amount of decanediamine and pentamethylenediamine accounts for more than 85%, further more than 90%, further more than 95% of the total amount of the diamine monomers, and the percentages are molar percentages.
[0012] As an embodiment of the present invention, the total amount of the aromatic dibasic acid and / or its derivatives and aliphatic dibasic acid accounts for more than 85%, further more than 90%, further more than 95% of the total amount of the diacid monomers, and the percentages are molar percentages.
[0013] As an embodiment of the present invention, the aromatic dibasic acid is any one or a combination of two or more of the dibasic acids containing benzene rings and having 8 or more carbon atoms, further including one or a combination of two or more of terephthalic acid, isophthalic acid, and phthalic acid. The aromatic dibasic acid derivatives include but are not limited to one or a combination of two or more of phthaloyl chloride, dimethyl terephthalate, and diethyl terephthalate.
[0014] The aliphatic dicarboxylic acid is any one of aliphatic diacids having 2 to 18 carbon atoms and a combination thereof, further including one or a combination of two or more of succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecane dicarboxylic acid, hexadecanedioic acid, heptadecanedioic acid and octadecane dicarboxylic acid.
[0015] As an embodiment of the present invention, the copolyamide is PA10T / 5T / 5X / 10X. The X represents a structural unit derived from an aliphatic dicarboxylic acid, and the aliphatic dicarboxylic acid has the same definition as described above.
[0016] As one embodiment of the present invention, the raw materials of the copolyamide also include additives accounting for 0.01% to 3% of the total mass of the monomers, and the additives include but are not limited to any one or a combination of two or more of end capping agents, catalysts, flame retardants, antioxidants, ultraviolet absorbers, infrared absorbers, crystallization nucleating agents, fluorescent brighteners and antistatic agents.
[0017] As an embodiment of the present invention, the raw material of the copolyamide further comprises 0.1% to 0.5% of the total weight of the monomers, and further 0.1% to 0.3% of the antioxidant. The antioxidant is selected from one or a combination of two or more of phenolic antioxidants, inorganic phosphate antioxidants, phosphite antioxidants and carbon free radical scavenger antioxidants.
[0018] As an embodiment of the present invention, the raw materials of the copolyamide further include a catalyst accounting for 0 to 0.07% of the total mass of the monomers, and further 0.005 to 0.05% of the catalyst. The catalyst includes phosphates and hypophosphites, and further includes phosphates of alkali metals and / or alkaline earth metals, hypophosphites of alkali metals and / or alkaline earth metals, and further includes one or a combination of two or more of potassium hypophosphite, sodium hypophosphite, calcium hypophosphite, magnesium hypophosphite, and zinc hypophosphite. Further, the total mass of the phosphates and hypophosphites accounts for more than 85% of the total mass of the catalyst, further more than 90%, and further more than 95%.
[0019] As one embodiment of the present invention, the raw material of the copolyamide also includes 0 to 1% of the total mass of the monomer end-capping agent, further 0.1 to 0.5% of the end-capping agent, and further 0.15% to 0.4% of the end-capping agent. The end-capping agent includes any one of C2 to C16 aliphatic carboxylic acids, C7 to C10 aromatic carboxylic acids, and combinations thereof. The structure of the aliphatic carboxylic acid end-capping agent is a linear, branched, or cyclic monoacid, and further a linear, branched, or cyclic saturated monoacid. The use of aliphatic carboxylic acids containing saturated cyclic structures has a better effect of reducing the YI value of the polymer than aliphatic carboxylic acids with a linear structure, mainly because aliphatic carboxylic acids with a cyclic structure have a larger steric hindrance effect, which can destroy the coplanarity of the atomic groups and reduce the degree of superposition of π electrons, thereby moving the absorption spectrum toward the short-wave direction.
[0020] Furthermore, the end-capping agent includes any one of C2-C10 aliphatic carboxylic acids, C7-C10 aromatic carboxylic acids, and combinations thereof. The number of carbon atoms in the end-capping agent is, for example, 3, 4, 5, 6, 7, 8, or 9.
[0021] Furthermore, the end-capping agent includes any one or a combination of two or more of acetic acid, propionic acid, butyric acid, valeric acid, hexanoic acid, octanoic acid, isobutyric acid, benzoic acid, cyclohexanecarboxylic acid, toluic acid, α-naphthoic acid, β-naphthoic acid, methylnaphthoic acid and phenylacetic acid.
[0022] Furthermore, the total mass of the C2-C10 aliphatic carboxylic acid and the C7-C10 aromatic carboxylic acid accounts for more than 85% of the total mass of the end-capping agent, further more than 90%, further more than 95%.
[0023] In some embodiments of the present invention, the melting point of the copolyamide is above 270°C, further 270°C to 310°C, for example 280°C, 290°C, 300°C, 305°C.
[0024] The relative viscosity of the copolyamide is 1.6 to 3.2, further 2.2 to 3.0, further 2.2 to 2.6, for example 2.3, 2.4, 2.5.
[0025] The water absorption of the copolyamide is 0.1-1%, further 0.2-0.8%, for example 0.4%, 0.6%, 0.7%.
[0026] The tensile strength of the copolyamide is 50 to 140 MPa, more preferably 60 to 120 MPa, further preferably 70 to 110 MPa, for example 80 MPa, 90 MPa, 95 MPa, 100 MPa, or 105 MPa.
[0027] In some embodiments of the present invention, the flexural strength of the copolyamide is 70 to 130 MPa, further 85 to 130 MPa, further 90 to 130 MPa, for example, 100 MPa, 105 MPa, 110 MPa, 115 MPa, 120 MPa, 125 MPa.
[0028] In some embodiments of the present invention, the heat deformation temperature of the copolyamide is 95-130°C, further 100-125°C, for example 105°C, 110°C, 115°C, 120°C.
[0029] In some embodiments of the present invention, the yellowness index YI value of the copolyamide is 15 or less, further 13 or less, further 10 or less, further 7 or less, for example, 2-7, 6, or 5.
[0030] After extensive research, the inventors found that amino groups are a type of auxochrome that can deepen the color of polymers containing chromogenic groups. The use of catalysts can reduce the concentration of terminal amino groups in polymers, increase the molecular weight of polymers, and obtain polymers with better mechanical properties and lower YI values.
[0031] In addition, for semi-aromatic polyamides containing long carbon chain structures, polymerization is prone to problems such as high polymer viscosity and poor melt fluidity. At present, in order to solve the problem of high polymer viscosity, the melt viscosity is generally reduced by increasing the temperature and shear rate, but the increase in temperature will promote the yellowing of the polymer. The addition of end-capping agents can adjust the viscosity of the polymer melt, reduce the cross-linking of the terminal amino groups under high temperature conditions, increase the fluidity of the polymer melt, and reduce the YI value of the polymer.
[0032] In another aspect, the present invention provides a method for preparing a high temperature resistant semi-aromatic copolyamide, the method comprising the following steps:
[0033] 1) adding decanediamine, pentamethylenediamine, aromatic dibasic acid and / or its derivatives, and aliphatic dicarboxylic acid to water, heating the water to 70-90° C., and optionally keeping the temperature at 70-90° C. for 0.5-3 hours to form a mixture containing polyamide salt;
[0034] 2) heating the mixture containing the polyamide salt to 120-140° C., draining and concentrating, and then heating to 240-255° C. for reaction;
[0035] 3) Exhaust pressure reduction.
[0036] Those skilled in the art know that the salt formed by the reaction of diamine and diacid is a polyamide salt (also known as nylon salt), and the polyamide salt is converted into polyamide or copolyamide through a polycondensation reaction.
[0037] In some embodiments of the present invention, the temperature increasing process in step 1) is carried out in an inert gas atmosphere; the inert gas includes one or more of nitrogen, argon or helium.
[0038] In some embodiments of the present invention, the insulation time in step 1) is 0.5 to 2 hours.
[0039] In some embodiments of the present invention, the drainage in step 2) is concentrated to a polyamide salt concentration of 40 wt% to 80 wt%, further 55 wt% to 65 wt%.
[0040] In some embodiments of the present invention, the reaction time in step 2) is 0.5 to 2 hours, further 1 to 1.5 hours;.
[0041] In some embodiments of the present invention, during the reaction in step 2), the pressure is maintained at 2.5-3 MPa.
[0042] In some embodiments of the present invention, the exhaust and pressure reduction in step 3) reduces the pressure in the reaction system to 0-0.2 MPa (gauge pressure).
[0043] In some embodiments of the present invention, the temperature of the reaction system after the pressure reduction in step 3) is 315-335°C.
[0044] In some embodiments of the present invention, the method further comprises step 4) vacuum treatment: vacuuming to a vacuum degree of less than -0.02 MPa, further to -0.05 MPa to -0.1 MPa. The vacuum treatment step before melt discharging can avoid the problem that a small amount of small molecules such as water still remain in the reaction system when the pressure drops to 0 in the pressure relief stage. In a high temperature environment, these remaining small molecules will cause the polymer to degrade, thereby affecting the performance of the material.
[0045] Optionally, the time for maintaining the above vacuum degree is 0 to 300 s, further 0 to 90 s, and further 5 to 90 s.
[0046] As an embodiment of the present invention, maintaining the vacuum degree within the above range is beneficial to the quality of the product. If the vacuum degree is maintained for a time significantly longer than the above time, the obtained copolyamide is difficult to melt and discharge for subsequent processing.
[0047] In some embodiments of the present invention, the method further comprises step 5): discharging, stranding and pelletizing.
[0048] In some embodiments of the present invention, the method further comprises adding an additive at any stage of step 1), step 2), step 3), and step 4). The additive has the same definition as described above.
[0049] As one embodiment of the present invention, the preparation method of the high temperature resistant semi-aromatic copolyamide comprises the following steps:
[0050] 1) adding decanediamine, pentamethylenediamine, aromatic dibasic acid and / or its derivatives, and aliphatic dicarboxylic acid into water, raising the temperature to 70-90° C., and keeping the temperature at 70-90° C. for 0.5-3 hours to form a mixture containing polyamide salt;
[0051] 2) heating the mixture containing the polyamide salt to 120-140° C., draining and concentrating the mixture to a concentration of 40 wt % to 80 wt % of the polyamide salt, heating the mixture to 240-255° C., maintaining the pressure at 2.5-3 MPa, and reacting the mixture for 0.5-2 h;
[0052] 3) exhausting and reducing the pressure in the reaction system to 0-0.2 MPa (gauge pressure), and the temperature of the reaction system after the pressure reduction is 315-335°C;
[0053] 4) Evacuate to a vacuum degree of -0.05 MPa to -0.1 MPa, and maintain the vacuum degree for 0 to 300 seconds;
[0054] 5) Discharging, stranding and pelletizing. The parameters of the method described are further limited as described above.
[0055] Another aspect of the present invention provides a composition, wherein the composition comprises any of the above-mentioned high temperature resistant semi-aromatic copolyamides.
[0056] Another aspect of the present invention provides a molded product prepared using the above-mentioned high temperature resistant semi-aromatic copolyamide as a raw material.
[0057] In order to obtain the molded article of the present invention, the copolyamide of the present invention can be molded by any molding method such as injection molding, extrusion molding, blow molding, vacuum molding, melt spinning, film molding, etc. These molded articles can be molded into a desired shape and can be used in resin molded articles such as automobile parts and machine parts.
[0058] Compared with the prior art, the implementation of the present invention has at least the following advantages:
[0059] 1. The copolyamide synthesized by the present invention has the same comprehensive performance as polyamide, and can use the monomer pentamethylenediamine developed with independent intellectual property rights, thus avoiding the use of the monomer hexamethylenediamine monopolized by foreign countries.
[0060] 2. The copolyamide synthesized by the present invention has excellent mechanical properties, and its tensile properties, bending resistance and impact resistance are comparable to those of polyamide products such as polyamide PA6 and polyamide PA66 used in the market.
[0061] 3. The copolyamide synthesized by the present invention has lower water absorption, better dimensional stability, higher heat deformation temperature and lower yellow index, and can be used in more demanding environments, thus expanding the application scope of polyamide to a certain extent.
[0062] 4. The preparation method of the copolyamide of the present invention is simple, the process parameters are easy to control, and no large-scale instrument assistance is required, which is convenient for quantitative production. DETAILED DESCRIPTION
[0063] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0064] 1. Detection method of relative viscosity ηr
[0065] Ubbelohde viscometer concentrated sulfuric acid method: Accurately weigh 0.5±0.0002 g of the dried polyamide sample, add 50 mL of concentrated sulfuric acid (98%) to dissolve it, and measure and record the concentrated sulfuric acid flow time t0 and the polyamide solution flow time t in a 25°C constant temperature water bath.
[0066] The formula for calculating relative viscosity is: relative viscosity ηr = t / t0, where: t: solution flow time; t0: solvent flow time.
[0067] 2. Mechanical properties test methods
[0068] The bending test is carried out according to ISO-178, and the test conditions are 2 mm / min.
[0069] The tensile test was carried out according to ISO-572-2, and the test conditions were 50 mm / min.
[0070] 3. Water absorption test: ISO-62:2008;
[0071] 4. Heat deformation temperature test: ASTM D648;
[0072] 5. Yellow index test
[0073] The yellow index is the yellow value based on the International Commission on Illumination (CIE) standard C light source and magnesium oxide as the benchmark. The calculation method of the yellow index YI is as follows:
[0074] YI=(100(1.28X-1.06Z)) / Y, wherein X, Y, and Z are the measured three stimulus values. A yellow index meter was used for detection, and the detection temperature was 25±5°C; the relative humidity was 50±20%.
[0075] Example 1
[0076] 9.45 mol of 1,10-decanediamine, 9.36 mol of terephthalic acid, 0.54 mol of 1,5-pentanediamine, 0.53 mol of adipic acid, 9.9 g of antioxidant H10, 7.83 g of end-capping agent acetic acid, 0.66 g of catalyst sodium hypophosphite and water were uniformly mixed, and the temperature was raised to 90° C. in a nitrogen atmosphere and maintained at the temperature for 1 hour to obtain a mixture containing polyamide salt, wherein the mass concentration of nylon salt in the mixture was 50 wt %;
[0077] The reaction system was heated to 130° C., and the water was drained and concentrated to a mass concentration of nylon salt of 65%; the temperature was raised to 250° C. again, and the pressure was maintained at 2.5 MPa for 1 hour; the pressure in the reaction system was reduced to 0 MPa (gauge pressure) by draining water, and the temperature of the reaction system was 335° C. After the pressure reduction, the vacuum degree was -0.07 MPa to obtain a copolyamide melt; the copolyamide melt was discharged and stretched and pelletized to obtain a high temperature resistant semi-aromatic copolyamide PA10T / 5T / 56 / 106.
[0078] Example 2
[0079] 9.09 mol of 1,10-decanediamine, 9 mol of terephthalic acid, 1.01 mol of 1,5-pentanediamine, 1 mol of adipic acid, 9.9 g of antioxidant H10, 7.83 g of end-capping agent benzoic acid, 0.66 g of catalyst sodium hypophosphite and water were mixed evenly, and the temperature was raised to 90° C. in a nitrogen atmosphere and maintained at the temperature for 1 hour to obtain a mixture containing polyamide salt, wherein the mass concentration of nylon salt in the mixture was 50 wt%.
[0080] The reaction system was heated to 130°C, and the water was drained and concentrated to a mass concentration of nylon salt of 65%; the temperature was raised to 250°C again, and the pressure was maintained at 2.5 MPa for 1 hour; the pressure in the reaction system was reduced to 0 MPa (gauge pressure), and the temperature of the reaction system was 325°C after the pressure reduction; the pressure was evacuated to -0.07 MPa, and the vacuum was maintained for 30 seconds to obtain a copolyamide melt; the copolyamide melt was discharged and stretched and pelletized to obtain a high temperature resistant semi-aromatic copolyamide PA10T / 5T / 56 / 106.
[0081] Example 3
[0082] 8.585 mol of 1,10-decanediamine, 8.5 mol of terephthalic acid, 1.5 mol of 1,5-pentanediamine, 1.5 mol of adipic acid, 9.8 g of antioxidant H10, 0.65 g of catalyst sodium hypophosphite, 7.83 g of end-capping agent acetic acid and water were uniformly mixed, and the temperature was raised to 90° C. in a nitrogen atmosphere and maintained at the temperature for 1 hour to obtain a mixture containing polyamide salt, wherein the mass concentration of nylon salt in the mixture was 50 wt%.
[0083] The reaction system was heated to 130°C, and the water was drained and concentrated to a mass concentration of nylon salt of 65%; the temperature was raised to 250°C again, and the pressure was maintained at 2.5 MPa for 1 hour; the pressure in the reaction system was reduced to 0 MPa (gauge pressure), and the temperature of the reaction system was 325°C after the pressure reduction; the pressure was evacuated to -0.07 MPa, and the vacuum was maintained for 30 seconds to obtain a copolyamide melt; the copolyamide melt was discharged and stretched and pelletized to obtain a high temperature resistant semi-aromatic copolyamide PA10T / 5T / 56 / 106.
[0084] Example 4
[0085] 8.08 mol of 1,10-decanediamine, 8 mol of terephthalic acid, 2.02 mol of 1,5-pentanediamine, 2 mol of adipic acid, 9.8 g of antioxidant H10, 0.66 g of catalyst calcium hypophosphite, 7.8 g of end-capping agent cyclohexanecarboxylic acid and water were mixed evenly, and the temperature was raised to 90° C. in a nitrogen atmosphere and maintained at the temperature for 1 hour to obtain a mixture containing polyamide salt, wherein the mass concentration of nylon salt in the mixture is 50 wt%.
[0086] The reaction system was heated to 130° C., and the water was drained and concentrated to a mass concentration of nylon salt of 65%; the temperature was raised to 250° C. again, and the pressure was maintained at 2.5 MPa for 1 hour; the pressure in the reaction system was reduced to 0 MPa (gauge pressure) by draining water, and the temperature of the reaction system was 325° C. The pressure was evacuated to -0.07 MPa, and the vacuum was maintained for 70 seconds to obtain a copolyamide melt; the copolyamide melt was discharged and stretched and pelletized to obtain a high temperature resistant semi-aromatic copolyamide PA10T / 5T / 56 / 106.
[0087] Example 5
[0088] The present embodiment 5 is basically the same as the embodiment 3, and the difference between the present embodiment 5 and the embodiment 3 is that the raw materials for preparing the copolyamide PA10T / 5T / 56 / 106 of the present embodiment 5 do not contain a catalyst.
[0089] Example 6
[0090] Basically the same as Example 3, the only difference between Example 6 and Example 3 is that the raw materials for preparing the copolyamide PA10T / 5T / 56 / 106 of Example 6 do not contain a capping agent.
[0091] Example 7
[0092] 8.08 mol of 1,10-decanediamine, 8 mol of terephthalic acid, 2.02 mol of 1,5-pentanediamine, 2 mol of dodecanedioic acid, 10.0 g of antioxidant H10, 0.70 g of catalyst sodium hypophosphite, 8.3 g of end-capping agent cyclohexanecarboxylic acid and water were mixed evenly, and the temperature was raised to 90° C. in a nitrogen atmosphere and maintained at the temperature for 1 hour to obtain a mixture containing polyamide salt, wherein the mass concentration of nylon salt in the mixture is 50 wt%.
[0093] The reaction system was heated to 130° C., and the water was drained and concentrated to a mass concentration of nylon salt of 65%; the temperature was raised to 250° C. again, and the pressure was maintained at 2.5 MPa for 1 hour; the pressure in the reaction system was reduced to 0 MPa (gauge pressure) by draining water, and the temperature of the reaction system was 325° C. The pressure was evacuated to -0.07 MPa, and the vacuum was maintained for 60 seconds to obtain a copolyamide melt; the copolyamide melt was discharged and stretched and pelletized to obtain a high temperature resistant semi-aromatic copolyamide PA10T / 5T / 512 / 1012.
[0094] Example 8
[0095] 8.585 mol of 1,10-decanediamine, 8.5 mol of terephthalic acid, 1.5 mol of 1,5-pentanediamine, 1.5 mol of hexadecanedioic acid, 10.2 g of antioxidant H10, 0.72 g of catalyst calcium hypophosphite, 8.2 g of end-capping agent acetic acid were mixed evenly with water, and the temperature was raised to 90° C. in a nitrogen atmosphere and maintained at the temperature for 1 hour to obtain a mixture containing polyamide salt, wherein the mass concentration of nylon salt in the mixture is 50 wt%.
[0096] The reaction system was heated to 130° C., and the water was drained and concentrated to a mass concentration of nylon salt of 65%; the temperature was raised to 250° C. again, and the pressure was maintained at 2.5 MPa for reaction for 1 hour; the pressure in the reaction system was reduced to 0 MPa (gauge pressure) by draining water, and the temperature of the reaction system was 325° C. The pressure was evacuated to -0.07 MPa, and the vacuum was maintained for 30 seconds to obtain a copolyamide melt; the copolyamide melt was discharged and stretched and pelletized to obtain a high temperature resistant semi-aromatic copolyamide PA10T / 5T / 516 / 1016.
[0097] Example 9
[0098] 8.585 mol of 1,10-decanediamine, 8.5 mol of terephthalic acid, 1.5 mol of 1,5-pentanediamine, 1.5 mol of adipic acid, 9.8 g of antioxidant H10, 0.65 g of catalyst sodium hypophosphite, 7.83 g of end-capping agent acetic acid and water were uniformly mixed, and the temperature was raised to 90° C. in a nitrogen atmosphere and maintained at the temperature for 1 hour to obtain a mixture containing polyamide salt, wherein the mass concentration of nylon salt in the mixture was 50 wt%.
[0099] The reaction system was heated to 130° C., and the water was drained and concentrated to a concentration of 65%; the temperature was raised to 250° C. again, and the pressure was maintained at 2.5 MPa for 1 hour; the pressure in the reaction system was reduced to 0 MPa (gauge pressure) by draining water, and the temperature of the reaction system was 325° C. after the pressure reduction, to obtain a copolyamide melt; the copolymer melt was discharged and subjected to stranding and pelletizing to obtain a high temperature resistant semi-aromatic copolyamide PA10T / 5T / 56 / 106.
[0100] Comparative Example 1
[0101] (1) Prepolymerization: 8.585 mol of 1,10-decanediamine, 8.5 mol of terephthalic acid, 1.5 mol of 1,5-pentanediamine, 1.5 mol of adipic acid, 9.8 g of an antioxidant, 0.65 g of a catalyst sodium hypophosphite, 7.83 g of an end-capping agent acetic acid and water were mixed uniformly, heated to 90° C. in a nitrogen atmosphere and maintained at the temperature for 1 hour to obtain a mixture containing a polyamide salt, wherein the mass concentration of nylon salt in the mixture was 50 wt %; the reaction system was heated to 130° C., and the water was drained and concentrated to a mass concentration of nylon salt of 65%; the temperature was again raised to 250° C., and the pressure was maintained at 2.5 MPa for 1 hour; the temperature was maintained at 250° C., the pressure in the reaction system was reduced to 0 MPa (gauge pressure), and the pressure was evacuated to -0.07 MPa for 30 seconds, and the reaction system was cooled to room temperature to obtain a solid prepolymer;
[0102] (2) Solid phase viscosity enhancement: The prepolymer was crushed into solid particles with a particle size of about 0.1 mm, placed in a vacuum drum for viscosity enhancement at 250° C. for 8 h, with a vacuum degree of 20-50 Pa, and then cooled to room temperature to obtain copolyamide PA10T / 5T / 56 / 106. The copolyamide resins prepared in Examples 1-9 and Comparative Example 1 were tested for relative viscosity, tensile strength, flexural strength, water absorption, heat deformation temperature, melting point, and yellowness index YI value. The test results are shown in Table 1.
[0103] Table 1
[0104]
[0105] As can be seen from Table 1, the examples all adopt a one-step method to prepare the copolyamide PA10T / 5T / 5X / 10X, which has the advantage of simple operation. Comparative Example 1 adopts a two-step method of prepolymerization followed by solid phase viscosity enhancement, which has low equipment utilization and complicated operation. By comparing Example 3 with Comparative Example 1, it can be seen that the improvement of prepolymerization viscosity by solid phase viscosity enhancement is very limited. At the same time, the YI value of the sample is much higher than that of the sample prepared by the one-step method, which may be caused by factors such as uneven heating of the sample in the solid phase viscosity enhancement equipment. The yellowing of the sample indicates that the sample has aged and degraded, so the mechanical properties are also reduced accordingly.
[0106] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A high temperature resistant semi-aromatic copolyamide, characterized in that: The monomer raw materials of the copolyamide include diacid monomers, diamine monomers, catalysts and end-capping agents, the diacid monomers include aromatic dibasic acids and / or derivatives thereof, aliphatic dibasic acids, the diamine monomers include decanediamine and pentamethylenediamine, and the molar ratio of decanediamine to pentamethylenediamine is (1-30):1; The catalyst accounts for 0.005-0.07% of the total mass of the monomers, the end-capping agent accounts for 0.1-1% of the total mass of the monomers, and the end-capping agent includes any one of C2-C16 aliphatic carboxylic acids, C7-C10 aromatic carboxylic acids, and combinations thereof; The water absorption rate of the copolyamide is 0.1-1%; the relative viscosity of the copolyamide is 2.2-3.0; and the yellowness index YI value of the copolyamide is less than 15.
2. The high temperature resistant semi-aromatic copolyamide according to claim 1, characterized in that: The 1,10-decanediamine in the monomer is 1,10-decanediamine of chemical or biological origin; and / or, The 1,5-pentanediamine in the monomer is pentamethylenediamine of chemical or biological origin; and / or, The molar ratio of decanediamine to aromatic dicarboxylic acid is 1:(0.7-1.5); and / or, The molar ratio of decanediamine to pentamethylenediamine is (2-30):1; and / or, The molar ratio of pentamethylenediamine to aliphatic dicarboxylic acid is (1-1.3):1; and / or, The molar ratio of the diamine monomer to the diacid monomer is (1-1.3):1; and / or, The total amount of the diamine monomer and the diacid monomer accounts for more than 85% of the total amount of monomer raw materials of the copolyamide; and / or, The total amount of decanediamine and pentamethylenediamine accounts for more than 85% of the total amount of the diamine monomers, and the percentage is molar percentage; and / or, The total amount of the aromatic dibasic acid and / or its derivatives and aliphatic dibasic acid accounts for more than 85% of the total amount of the diacid monomers, and the percentage is molar percentage; and / or, The copolyamide is PA10T / 5T / 5X / 10X.
3. The high temperature resistant semi-aromatic copolyamide according to claim 2, characterized in that: The molar ratio of decanediamine to aromatic dicarboxylic acid is 1:(0.8-1.2); and / or, The molar ratio of decanediamine to pentamethylenediamine is (2-30):1; and / or, The molar ratio of pentamethylenediamine to aliphatic dicarboxylic acid is (1-1.1):1; and / or, The molar ratio of the diamine monomer to the diacid monomer is (1-1.1):1; and / or, The total amount of the diamine monomer and the diacid monomer accounts for more than 90% of the total amount of the monomer raw materials of the copolyamide, and the percentage is a molar percentage; and / or, The total amount of decanediamine and pentamethylenediamine accounts for more than 90% of the total amount of the diamine monomers, and the percentage is molar percentage; and / or, The total amount of the aromatic dibasic acid and / or its derivatives and the aliphatic dibasic acid accounts for more than 90% of the total amount of the diacid monomers, and the percentage is a molar percentage.
4. The high temperature resistant semi-aromatic copolyamide according to claim 3, characterized in that: The molar ratio of decanediamine to pentamethylenediamine is (2-20):1; and / or, The molar ratio of pentamethylenediamine to aliphatic dicarboxylic acid is (1-1.06):1; and / or, The molar ratio of the diamine monomer to the diacid monomer is (1-1.06):1; and / or, The total amount of the diamine monomer and the diacid monomer accounts for more than 95% of the total amount of the monomer raw materials of the copolyamide, and the percentage is a molar percentage; and / or, The total amount of decanediamine and pentamethylenediamine accounts for more than 95% of the total amount of the diamine monomers, and the percentage is molar percentage; and / or, The total amount of the aromatic dibasic acid and / or its derivatives and the aliphatic dibasic acid accounts for more than 95% of the total amount of the diacid monomers, and the percentage is a molar percentage.
5. The high temperature resistant semi-aromatic copolyamide according to claim 4, characterized in that: The molar ratio of the diamine monomer to the diacid monomer is (1.01-1.04):1; and / or, The total amount of the diamine monomer and the diacid monomer accounts for more than 97% of the total amount of monomer raw materials of the copolyamide.
6. The high temperature resistant semi-aromatic copolyamide according to claim 1, characterized in that: The aromatic dibasic acid is any one or a combination of two or more dibasic acids having a benzene ring and having 8 or more carbon atoms; and / or, The aromatic dibasic acid derivative includes one or a combination of two or more of terephthaloyl chloride, dimethyl terephthalate and diethyl terephthalate; and / or, The aliphatic dicarboxylic acid is any one of aliphatic diacids having 2 to 18 carbon atoms and a combination thereof.
7. The high temperature resistant semi-aromatic copolyamide according to claim 6, characterized in that: The aromatic dibasic acid is one of terephthalic acid, isophthalic acid, and phthalic acid, or a combination of two or more thereof; and / or, The aliphatic dicarboxylic acid is one or a combination of two or more of the following: succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedicarboxylic acid, hexadecanedioic acid, heptadecanedioic acid, and octadecanedicarboxylic acid.
8. The high temperature resistant semi-aromatic copolyamide according to claim 1, characterized in that: The raw materials of the copolyamide include additives accounting for 0.01% to 3% of the total weight of the monomers, and the additives include the end-capping agent, the catalyst, and any one or a combination of two or more of a flame retardant, an antioxidant, an ultraviolet absorber, an infrared absorber, a crystal nucleating agent, a fluorescent brightener, and an antistatic agent; and / or, The raw materials of the copolyamide further include 0.1% to 0.5% of the total weight of the monomers as antioxidant, wherein the antioxidant includes one or a combination of two or more of phenolic antioxidants, inorganic phosphate antioxidants, phosphite antioxidants and carbon free radical scavenger antioxidants; and / or, The raw materials of the copolyamide include 0.005-0.05% of the total weight of the monomers as catalyst, and the catalyst includes phosphate and hypophosphite; and / or, The raw materials of the copolyamide include 0.1-0.5% of the total weight of the monomers as the end-capping agent.
9. The high temperature resistant semi-aromatic copolyamide according to claim 8, characterized in that: The catalyst comprises phosphates of alkali metals and / or alkaline earth metals, hypophosphites of alkali metals and / or alkaline earth metals; and / or The end-capping agent includes any one of C2-C10 aliphatic carboxylic acids, C7-C10 aromatic carboxylic acids, and combinations thereof.
10. The high temperature resistant semi-aromatic copolyamide according to claim 9, characterized in that: The catalyst comprises one or a combination of two or more of potassium hypophosphite, sodium hypophosphite, calcium hypophosphite, magnesium hypophosphite and zinc phosphite; and / or The end-capping agent includes any one or a combination of two or more of acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, octanoic acid, trimethylacetic acid, isobutyric acid, benzoic acid, cyclohexanecarboxylic acid, toluic acid, α-naphthoic acid, β-naphthoic acid, methylnaphthoic acid and phenylacetic acid.
11. The high temperature resistant semi-aromatic copolyamide according to any one of claims 1 to 10, characterized in that The melting point of the copolyamide is above 270° C.; and / or, The heat deformation temperature of the copolyamide is 95 to 130° C.; and / or, The tensile strength of the copolyamide is 50 to 140 MPa; and / or, The flexural strength of the copolyamide is 70 to 130 MPa.
12. The high temperature resistant semi-aromatic copolyamide according to claim 11, characterized in that: The melting point of the copolyamide is 270° C. to 310° C.; and / or, The heat deformation temperature of the copolyamide is 100 to 125° C.; and / or, The water absorption rate of the copolyamide is 0.2 to 0.8%; and / or, The tensile strength of the copolyamide is 60 to 120 MPa; and / or, The flexural strength of the copolyamide is 85 to 130 MPa; and / or, The yellowness index YI value of the copolyamide is 13 or less.
13. The high temperature resistant semi-aromatic copolyamide according to claim 12, characterized in that: The relative viscosity of the copolyamide is 2.2 to 2.6; and / or, The tensile strength of the copolyamide is 70 to 110 MPa; and / or, The flexural strength of the copolyamide is 90 to 130 MPa; and / or, The yellowness index YI value of the copolyamide is 10 or less.
14. The high temperature resistant semi-aromatic copolyamide according to claim 13, characterized in that: The yellowness index YI value of the copolyamide is 7 or less.
15. A method for preparing a high temperature resistant semi-aromatic copolyamide, characterized in that: The method comprises the following steps: 1) adding decanediamine, pentamethylenediamine, aromatic dibasic acid and / or its derivatives, and aliphatic dicarboxylic acid to water, raising the temperature to 70-90° C., and keeping the temperature at 70-90° C. for 0.5-3 hours to form a mixture containing polyamide salt; 2) heating the mixture containing the polyamide salt to 120-140° C., draining and concentrating, and then heating to 240-255° C. for reaction; 3) Exhaust pressure reduction; wherein at any stage of steps 1) and 2), a catalyst accounting for 0.005-0.07% of the total mass of the monomer and a capping agent accounting for 0.1-1% of the total mass of the monomer are added, wherein the capping agent includes any one of C2-C16 aliphatic carboxylic acids, C7-C10 aromatic carboxylic acids, and combinations thereof; The water absorption rate of the copolyamide is 0.1-1%; the relative viscosity of the copolyamide is 2.2-3.0; and the yellowness index YI value of the copolyamide is less than 15.
16. The method according to claim 15, characterized in that The temperature raising process in step 1) is carried out in an inert gas atmosphere; and / or, The holding time in step 1) is 0.5 to 2 hours; and / or, Step 2) the drainage is concentrated to a polyamide salt concentration of 40 wt% to 80 wt%; and / or, Step 2) The reaction is carried out for 0.5 to 2 hours; and / or, Step 2) During the reaction, the pressure is maintained at 2.5-3 MPa; and / or, Step 3) the exhaust and pressure reduction is performed to reduce the pressure in the reaction system to a gauge pressure of 0 to 0.2 MPa; and / or, Step 3) After the pressure reduction is completed, the temperature of the reaction system is 315-335° C.; and / or, The method comprises the following steps: vacuumizing the device to a vacuum degree of -0.02 MPa or less, and maintaining the vacuum degree for 0 to 300 seconds; and / or The method comprises step 5): discharging the material, and cutting the material into strands and pelletizing the pellets.
17. The method according to claim 16, characterized in that Step 2) the drainage is concentrated to a concentration of 55wt% to 65wt% of the polyamide salt; and / or, Step 2) The reaction is carried out for 1 to 1.5 hours; and / or, Step 4): vacuum treatment: vacuuming to a vacuum degree of -0.05 MPa to -0.1 MPa, and maintaining the vacuum degree for 0 to 300 seconds; and / or, The method comprises step 5): discharging the material, and cutting the material into strands and pelletizing the pellets.
18. The method according to claim 17, characterized in that Step 4) The holding time is 0 to 90 seconds.
19. The method according to claim 18, characterized in that Step 4) is maintained for 5 to 90 seconds.
20. The method according to claim 15, characterized in that Additives are added at any stage of steps 1), 2), 3) and 4), and the additives account for 0.01% to 3% of the total mass of the monomers. The additives include any one or a combination of two or more of the capping agent, the catalyst, and flame retardants, antioxidants, ultraviolet absorbers, infrared absorbers, crystal nucleating agents, fluorescent brighteners and antistatic agents.
21. A composition, characterized in that The invention comprises the high temperature resistant semi-aromatic copolyamide according to any one of claims 1 to 14.
22. A molded article prepared using the high temperature resistant semi-aromatic copolyamide according to any one of claims 1 to 14 as a raw material.