A thermal sublimation ribbon capable of maintaining high color density under high-speed printing and a high-speed printing substrate

By using a PET film base, a wear-resistant thermal transfer back coating and an optimized dye layer combination in the dye-sublimation ribbon, the color density reduction and bonding problems of traditional dye-sublimation ribbons during high-speed printing are solved, achieving high-speed printing. High color density and continuous printing at high speed.

CN115635785BActive Publication Date: 2024-10-25HUNAN DINGYIYUAN TECH DEV CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211190211.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-28
Publication Date
2024-10-25
Estimated Expiration
2042-09-28

AI Technical Summary

Technical Problem

The color density of traditional dye-sublimation ribbons decreases during high-speed printing. The back coating resin melts and falls off, causing damage to the print head. The base material has insufficient heat resistance and cannot maintain high color density and continuous printing.

Method used

The sublimation ribbon is made of PET film base, coated with wear-resistant thermal transfer back coating, adhesive layer and dye layer to increase the smoothness and heat resistance of the dye layer. Polyvinylpyrrolidone and other resins are used, and silicone oil and Solid lubricant, optimizes coating thickness and proportion, and adapts to the printing layer design of different substrates.

Benefits of technology

Maintain high color density at a high-speed printing speed of 6-10m/min, avoid the adhesion of the ribbon and the substrate, and ensure printing quality and equipment safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115635785B_ABST
    Figure CN115635785B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of thermal sublimation printing, and specifically relates to a thermal sublimation ribbon and a high-speed printing substrate that maintain high color density under high-speed printing. The thermal sublimation ribbon that maintains high color density under high-speed printing includes a back coating, a substrate, an adhesive layer and a dye layer that are arranged in sequence, or includes a back coating, a substrate and a dye layer that are arranged in sequence. The thermal sublimation ribbon can maintain a high color density at a printing speed of 6-10m / min, and at the same time, because it is coated with a back coating with good heat resistance, it can maintain continuous printing at high speed without breaking the film. The thermal sublimation carbon ribbon and the matching substrate have very good surface smoothness, so that the substrate and the ribbon will not be bonded during continuous printing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal sublimation printing, and in particular relates to a thermal sublimation ribbon and a high-speed printing substrate which can maintain high color density under high-speed printing. Background Art

[0002] Thermal sublimation printing technology is often used to replace traditional photo printing because it can achieve continuous color gradation printing. Generally speaking, there are several problems when traditional thermal sublimation ribbons are directly used for packaging material printing: 1. When the printing speed exceeds 2m / min, the color density of thermal sublimation printing decreases significantly. 2. Packaging printing requires continuous printing. Traditional thermal sublimation ribbons are mainly used for photo printing. If they are directly used for continuous printing, the back coating resin will melt and fall off and adhere to the print head, resulting in uneven heat transfer, causing obvious color difference in the printed pattern, and even causing the print head to burn out in severe cases. 3. If traditional thermal sublimation ribbons are directly used for packaging printing, in order to obtain high color density at high-speed printing, the printing heat and pressure need to be increased, which will cause the dye layer and the printing layer to melt and bond. At the same time, the back coating will also break due to insufficient heat resistance. 4. The packaging substrates on the market cannot be used as the substrate of thermal sublimation ribbons. The processed ones, such as thermal sublimation printing photo paper, also have the problem of heat resistance at high-speed printing. Summary of the invention

[0003] In order to solve the shortcomings of the prior art, the present invention provides a thermal sublimation ribbon and a substrate that can maintain high color density under high-speed printing. The thermal sublimation ribbon can maintain a high color density at a printing speed of 6-10m / min. At the same time, because it is coated with a back coating with good heat resistance, it can maintain continuous printing at high speed without breaking the film. The thermal sublimation ribbon and the matching substrate have very good surface smoothness, so that the substrate and the ribbon will not stick together during continuous printing.

[0004] The technical solution provided by the present invention is as follows:

[0005] A thermal sublimation ribbon which maintains high color density under high-speed printing comprises a back coating layer, a substrate, a bonding layer and a dye layer which are arranged in sequence, or comprises a back coating layer, a substrate and a dye layer which are arranged in sequence.

[0006] As for the base material of thermal sublimation ribbon:

[0007] The color ribbon of the present invention comprises a PET film substrate, the upper side of the substrate is provided with a wear-resistant heat transfer back coating layer, and the lower side of the PET substrate is provided with two coating layers: an adhesive layer and a dye layer in sequence.

[0008] Furthermore, the thickness of the substrate is 4-125 μm, and the substrate is composed of a PET film. Preferably, the thickness of the PET film substrate is 4.3-12.5 μm.

[0009] Generally speaking, the substrate needs to be surface treated before coating is applied directly on the substrate. Considering the cost, corona discharge treatment is generally used to make the dyne value of the substrate surface greater than 38.

[0010] As for the adhesive layer material of thermal sublimation ribbon:

[0011] The effect of the bonding layer is mainly to increase the bonding property of the dye layer and the substrate, so that the dye layer will not fall off and cause abnormal discoloration due to poor adhesion during printing. But at the same time, the dye will diffuse in two opposite directions of the substrate and the bonding layer at the same time when heated, so the bonding layer preferably selects a resin or sol that satisfies poor dye adsorption and excellent adhesion on the substrate at the same time. For coating considerations, it is preferred to use one or more of polyvinyl pyrrolidone, polyvinyl alcohol, polyvinyl acetal, polyvinyl butyral, methyl cellulose, etc. The thickness is 0.1-0.5 μm, and the preferred thickness is 0.1-0.3 μm. If the coating thickness is too low or too high, there is a risk of printing discoloration.

[0012] An adhesive layer may or may not be provided.

[0013] As for the dye layer material of thermal sublimation ribbon:

[0014] The function of the dye layer is mainly to provide dyes for true color printing. There is no particular limitation on the dyes, and the dyes can be selected from a variety of sublimation dyes. Since the ribbon needs to be used under high-speed printing, dyes with low melting and sublimation temperatures and good solubility are preferred. As a binder for the dyes, the main resin of the dye layer preferably uses one or more of polyvinyl pyrrolidone, polyvinyl alcohol, polyvinyl acetal, polyvinyl butyral, methyl cellulose, polyurethane, polycarbonate, polyester resin, etc., and the solvent uses a mixture of butanone and toluene in a ratio of 1:1.

[0015] The dye can be a common solvent-based thermal sublimation dye such as indole aniline dye, pyridone azo dye, arylmethane dye, pyridine dye, etc. There is no special restriction on the type and amount of the dye, and the light reflection density after printing is greater than 1.8.

[0016] The present invention makes the following improvements to the dye layer:

[0017] Furthermore, in order to maximize the color density of printing under high-speed printing, the ratio of dye to resin needs to be increased as much as possible, and the preferred ratio is (1:0.8)-(1:0.6). If the dye content is too high, the risk of color fading will increase, and if the dye content is too low, the color density of printing will decrease significantly.

[0018] Furthermore, in order to adapt the ribbon to the high heat and high pressure required for high-speed printing, reduce the transfer of liquid lubricant on the substrate to the ribbon, and prevent the ribbon from sticking to the substrate during printing, the smoothness of the dye layer needs to be increased. A certain amount of silicone oil can be added to the dye layer to increase the smoothness of the ribbon surface. Considering that the dye layer will directly contact the back coating when the ribbon is rolled up, non-reactive silicone oil is preferred to reduce the loss of lubricant in the dye layer. The content of silicone oil is 0.1-5phr of the resin.

[0019] Furthermore, in order to make the ribbon maintain good printing quality after being exposed to high temperature and high humidity environment, and to prevent the dye layer from bonding with the back coating layer, a certain amount of solid lubricant can be added to the dye layer. The preferred lubricant is PE wax or sol, and the sol is mainly silica sol and alumina sol. The preferred amount is 0.5-1.5phr of the resin. The amount needs to be well controlled. If too much is added, the print color density will be reduced, and if too little is added, the back coating layer may bond with the dye layer.

[0020] Furthermore, in order to adapt the ribbon to the high heat and high pressure under high-speed printing, a certain amount of isocyanate curing agent can be added to the dye layer to improve the heat resistance, adhesion and bonding strength of the dye layer. The content is 1-10 phr of the resin.

[0021] The recommended coating thickness of the dye layer is 0.5-1.5 μm, and the preferred thickness is 0.7-1.2 μm.

[0022] As for the back coating of the sublimation ribbon:

[0023] Wear-resistant heat transfer back coating composition mainly contains heat-resistant resin, generally uses one or more of polyvinyl butyral resin, polyvinyl acetal resin, polyester resin, polyurethane resin, polycarbonate resin, cellulose acetate butyrate, etc., preferably uses one or both of polyvinyl butyral resin and cellulose acetate. In this coating, generally also a certain amount of liquid lubricant is added to reduce the friction force when the coating contacts with the thermal print head, to achieve the effect of protecting the print head. Generally use silicone oil as back coating slip agent, preferably use silicone oil that can migrate to the surface, and the addition amount is 0.5-5phr of resin, and the preferred addition amount is 1-3phr. To prevent the back coating from bonding with the dye layer under high temperature and high humidity environment, a certain amount of solid lubricant also needs to be added, considering the high heat under high-speed printing, preferably one or more of phosphate, zinc stearate, silicone resin particles, talcum powder, etc., and the addition amount is generally 0.5-10phr of resin, and the preferred addition amount is 1-5phr.

[0024] The recommended coating thickness of the heat-resistant back coating layer is 0.3-1.5 μm, and the preferred coating thickness is 0.3-0.7 μm.

[0025] The present invention also provides a high-speed printing substrate:

[0026] According to the characteristics of different printing substrates, the present invention provides different printing layer designs:

[0027] For paper substrates, a white or transparent base coating is generally applied to the surface in contact with the substrate, and then a printing layer is disposed thereon.

[0028] For plastic substrates, a transparent base coating is generally applied on the surface in contact with the substrate, and then a printing layer is arranged thereon.

[0029] Regarding the substrate material for high-speed printing:

[0030] For paper or plastic substrates, the composition of the printing layer is basically the same. The main resin is preferably a halogenated resin such as polyvinyl chloride or polyvinylidene chloride and a vinyl chloride-vinyl acetate copolymer, preferably a vinyl chloride-vinyl acetate copolymer, and the ratio of vinyl chloride to vinyl acetate is in the range of 80:20-90:10.

[0031] In order to prevent the problem of adhesion between the substrate and the ribbon due to melting of the resin caused by heating during the printing process, a certain amount of anti-sticking agent needs to be added to the substrate to prevent adhesion. Because the substrate is in close contact with the ribbon during thermal sublimation printing, the liquid lubricant in the substrate will gradually migrate to the surface of the ribbon, and the substrate at the same position must contact the ribbon three times, which will increase the risk of adhesion between the substrate and the ribbon step by step. In order to solve this problem, the present invention adopts the following scheme: adding a certain amount of reactive silicone oil and curing agent, the added amount is 0.5-1.5phr of the resin to fix the silicone oil and the main resin through reaction, increase the closeness and adhesion of the substrate, and reduce the thermal migration of the silicone oil. The recommended coating thickness of the substrate is 5-15μm, and the preferred thickness is 6-10μm.

[0032] For paper base coatings for high-speed printing substrates:

[0033] The main function of the primer layer for paper substrates is to smooth the rough surface and improve the flatness of the printing layer, thereby improving the uniformity of the printed image. Generally, the optional resins are polyester resins, polyurethane resins, polycarbonate resins and acrylic resins, and the preferred resin is polyurethane resin. Further, in order to improve the brightness of the printing layer, a certain amount of rutile titanium dioxide and fluorescent brightener can be added to the primer layer. The amount of titanium dioxide added is 80-120% of the resin, and the amount of fluorescent brightener added is 0.05-0.1% of the total amount of titanium dioxide and resin. Further, in order to reduce the diffusion of heat into the interior of the substrate during transfer, a certain amount of thermal insulation material can be added to the primer layer. The preferred thermal insulation material is hollow microspheres or foamed resin, and its particle size is preferably 1-5μm. The recommended coating thickness is 2-10μm, and the preferred thickness is 2-5μm. Its addition amount is 80-120wt% of the resin.

[0034] Regarding plastic base coating materials for high-speed printing substrates:

[0035] The main function of the primer layer for plastic substrates is to improve the adhesion between the printing layer and the substrate. For PET substrates, the substrate thickness is generally 50-150μm, preferably 50-75μm. The main resin of the primer layer of the PET substrate can be selected from polyester resin, polyurethane resin, acrylic resin, polycarbonate resin, etc., preferably polyester resin or polyurethane resin. Polyurethane resin is particularly preferred. Due to the problem of water absorption and shrinkage of polyurethane resin, a certain amount of anti-hydrolysis agent and curing agent needs to be added, and the added amount is preferably 1-5% of the resin. For PP substrates, the substrate thickness is generally 50-150μm, preferably 50-100μm. The main resin of the primer layer of the PP substrate can be selected from one or more of polyester resin, chlorinated polypropylene resin, and polyurethane. For plastic substrates, considering cost and performance, the thickness of the primer layer should not be too thick, and the preferred coating thickness is 1-3μm.

[0036] The invention provides a thermal sublimation ribbon and a high-speed printing substrate which can maintain high color density under high-speed printing, and can increase the printing speed of the thermal sublimation ribbon to 6-10 m / min while maintaining high color density of printing. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 The present invention is a schematic structural diagram of a thermal sublimation ribbon that maintains high color density under high-speed printing.

[0038] Attached Figure 1 The structures represented by the labels are listed below:

[0039] 1. Back coating layer, 2. PET substrate, 3. Adhesive layer, 4. Dye layer. DETAILED DESCRIPTION

[0040] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0041] Sublimation ribbon example 1:

[0042] Considering the high heat under high-speed printing, the substrate uses a 6μm thick PET film, and the manufacturer is Anhui Tongai.

[0043] <Bonding layer>:

[0044] Polyvinyl pyrrolidone (industrial grade PVP K90 Guangdong Yuemei Chemical) 2 parts

[0045] Polyvinyl alcohol (Tianjin Damao Chemical) 1 part

[0046] Silica sol (HS830 Guangdong Huierte Nanotechnology) 1 part

[0047] 48 parts water

[0048] 48 parts of isopropyl alcohol

[0049] The coating was performed using a gravure coater, and the coating thickness was 0.2 μm.

[0050] <Dye Layer>:

[0051] yellow:

[0052] Polyurethane (901H Wanhua Chemical) 4.5 parts

[0053] Solvent Yellow 2 (Henan Wokas Biotechnology) 5.5 parts

[0054] Silicone oil (KM-244F Shin-Etsu silicone) 0.02 parts

[0055] Isocyanate ( Wanhua Chemical) 0.5 parts

[0056] 2-Butanone 44.5 parts

[0057] Toluene 44.5 parts

[0058] Magenta:

[0059] Polyurethane (901H Wanhua Chemical) 4.5 parts

[0060] Solvent Red 24 (Sinopharm Chemical Reagent) 5.5 parts

[0061] Silicone oil (KM-244F Shin-Etsu silicone) 0.03 parts

[0062] Isocyanate ( Wanhua Chemical) 0.5 parts

[0063] 2-Butanone 44.5 parts

[0064] Toluene 44.5 parts

[0065] blue:

[0066] Polyurethane (901H Wanhua Chemical) 4.5 parts

[0067] Solvent Blue 36 (Nanjing Kangmanlin Chemical Industry) 5.5 parts

[0068] Silicone oil (KM-244F Shin-Etsu silicone) 0.05 parts

[0069] Isocyanate ( Wanhua Chemical) 0.5 parts

[0070] 2-Butanone 44.5 parts

[0071] Toluene 44.5 parts

[0072] The coating was performed using a gravure coater with a coating thickness of 1.0 μm.

[0073] <Back coating>:

[0074] 3 parts of polyvinyl butyral (B265H-B Guangzhou Hongshang)

[0075] Cellulose acetate butyrate (CAB393-3 American Eastman) 7 parts

[0076] Isocyanate ( Wanhua Chemical) 5 copies

[0077] Glycerol phosphate (Guangzhou Jiatu Technology) 0.3 parts

[0078] Zinc stearate (Henan Xinzhiyuan Chemical) 0.3 parts

[0079] Talc (LJ-320 Liangjiang Chemical) 0.3 parts

[0080] Polyethylene wax (3405G Honeywell) 0.5 parts

[0081] Silicone oil (KF-6001 Shin-Etsu silicone) 0.2 parts

[0082] 2-Butanone 58 parts

[0083] Toluene 25.4 parts

[0084] The coating was performed using a gravure coater, and the coating thickness was 0.6 μm.

[0085] Sublimation ribbon example 2:

[0086] Considering the high heat under high-speed printing, the substrate uses a 6μm thick PET film, and the manufacturer is Anhui Tongai.

[0087] <Bonding layer>:

[0088] Polyvinyl pyrrolidone (industrial grade PVP K90 Guangdong Yuemei Chemical) 2 parts

[0089] Polyvinyl alcohol (Tianjin Damao Chemical) 1 part

[0090] Alumina sol (WN-AH03 ultra-micro nano new material) 1 part

[0091] 48 parts water

[0092] 48 parts of isopropyl alcohol

[0093] The coating was performed using a gravure coater, and the coating thickness was 0.2 μm.

[0094] <Dye Layer>:

[0095] yellow:

[0096] Polyurethane (901H Wanhua Chemical) 4.5 parts

[0097] Solvent Yellow 2 (Henan Wokas Biotechnology) 5.5 parts

[0098] Silicone oil (KM-244F Shin-Etsu silicone) 0.02 parts

[0099] Isocyanate ( Wanhua Chemical) 0.5 parts

[0100] 2-Butanone 44.5 parts

[0101] Toluene 44.5 parts

[0102] Magenta:

[0103] Polyurethane (901H Wanhua Chemical) 4.5 parts

[0104] Solvent Red 24 (Sinopharm Chemical Reagent) 5.5 parts

[0105] Silicone oil (KM-244F Shin-Etsu silicone) 0.03 parts

[0106] Isocyanate ( Wanhua Chemical) 0.5 parts

[0107] 2-Butanone 44.5 parts

[0108] Toluene 44.5 parts

[0109] blue:

[0110] Polyurethane (901H Wanhua Chemical) 4.5 parts

[0111] Solvent Blue 36 (Nanjing Kangmanlin Chemical Industry) 5.5 parts

[0112] Silicone oil (KM-244F Shin-Etsu silicone) 0.05 parts

[0113] Isocyanate ( Wanhua Chemical) 0.5 parts

[0114] 2-Butanone 44.5 parts

[0115] Toluene 44.5 parts

[0116] The coating was performed using a gravure coater with a coating thickness of 1.0 μm.

[0117] <Back coating>:

[0118] 3 parts of polyvinyl butyral (B265H-B Guangzhou Hongshang)

[0119] Cellulose acetate butyrate (CAB393-3 American Eastman) 7 parts

[0120] Isocyanate ( Wanhua Chemical) 5 copies

[0121] Glycerol phosphate (Guangzhou Jiatu Technology) 0.3 parts

[0122] Zinc stearate (Henan Xinzhiyuan Chemical) 0.3 parts

[0123] Talc (LJ-320 Liangjiang Chemical) 0.3 parts

[0124] Polyethylene wax (3405G Honeywell) 0.5 parts

[0125] Silicone oil (KF-6001 Shin-Etsu silicone) 0.2 parts

[0126] 2-Butanone 58 parts

[0127] Toluene 25.4 parts

[0128] The coating was performed using a gravure coater, and the coating thickness was 0.6 μm.

[0129] Sublimation ribbon example 3:

[0130] The substrate, adhesive layer and back coating are consistent with those in Example 1, and the dye layer formula is as follows:

[0131] yellow:

[0132] Polyurethane (901H Wanhua Chemical) 4 parts

[0133] Solvent Yellow 2 (Henan Wokas Biotechnology) 6 parts

[0134] Silicone oil (KM-244F Shin-Etsu silicone) 0.02 parts

[0135] Isocyanate ( Wanhua Chemical) 0.5 parts

[0136] 2-Butanone 44.5 parts

[0137] Toluene 44.5 parts

[0138] Magenta:

[0139] Polyurethane (901H Wanhua Chemical) 4 parts

[0140] Solvent Red 24 (Sinopharm Group Chemical Reagent) 6 parts

[0141] Silicone oil (KM-244F Shin-Etsu silicone) 0.03 parts

[0142] Isocyanate ( Wanhua Chemical) 0.5 parts

[0143] 2-Butanone 44.5 parts

[0144] Toluene 44.5 parts

[0145] blue:

[0146] Polyurethane (901H Wanhua Chemical) 4 parts

[0147] Solvent Blue 36 (Nanjing Kangmanlin Chemical Industry) 6 parts

[0148] Silicone oil (KM-244F Shin-Etsu silicone) 0.05 parts

[0149] Isocyanate ( Wanhua Chemical) 0.5 parts

[0150] 2-Butanone 44.5 parts

[0151] Toluene 44.5 parts

[0152] The coating was performed using a gravure coater with a coating thickness of 1.0 μm.

[0153] Sublimation ribbon example 4:

[0154] The substrate, adhesive layer and back coating are the same as those in Example 2, and the dye layer is the same as that in Example 3.

[0155] Sublimation ribbon example 5:

[0156] The adhesive layer and dye layer are consistent with Example 1, and the back coating formula is as follows:

[0157] 3 parts of polyvinyl butyral (B265H-B Guangzhou Hongshang)

[0158] Cellulose acetate butyrate (CAB393-3 American Eastman) 7 parts

[0159] Isocyanate ( Wanhua Chemical) 5 copies

[0160] Glycerol phosphate (Guangzhou Jiatu Technology) 0.3 parts

[0161] Zinc stearate (Henan Xinzhiyuan Chemical) 0.3 parts

[0162] 0.3 parts of silicone resin particles (KMP-590 Shin-Etsu silicone)

[0163] Polyethylene wax (3405G Honeywell) 0.5 parts

[0164] Silicone oil (KF-6001 Shin-Etsu silicone) 0.2 parts

[0165] 2-Butanone 58 parts

[0166] Toluene 25.4 parts

[0167] Coating thickness 0.6μm.

[0168] Sublimation ribbon example 6:

[0169] The adhesive layer and dye layer are consistent with Example 2, and the back coating formulation is consistent with Example 5.

[0170] Sublimation ribbon example 7:

[0171] The formulations of the adhesive layer, dye layer and back coating layer are consistent with those in Example 1, and the thickness of the dye layer is changed to 1.2 μm.

[0172] Sublimation ribbon example 8:

[0173] The adhesive layer, dye layer and back coating formulations are consistent with Junyu Example 7, and the back coating thickness is changed to 0.3 μm.

[0174] Sublimation ribbon comparison example 1:

[0175] The adhesive layer and back coating are consistent with Example 1, and the dye layer formula is as follows:

[0176] yellow:

[0177] Polyurethane (901H Wanhua Chemical) 4.5 parts

[0178] Solvent Yellow 2 (Henan Wokas Biotechnology) 5.5 parts

[0179] Silicone oil (KM-244F Shin-Etsu silicone) 0.02 parts

[0180] 2-Butanone 44.5 parts

[0181] Toluene 44.5 parts

[0182] Magenta:

[0183] Polyurethane (901H Wanhua Chemical) 4.5 parts

[0184] Solvent Red 24 (Sinopharm Chemical Reagent) 5.5 parts

[0185] Silicone oil (KM-244F Shin-Etsu silicone) 0.03 parts

[0186] 2-Butanone 44.5 parts

[0187] Toluene 44.5 parts

[0188] blue:

[0189] Polyurethane (901H Wanhua Chemical) 4.5 parts

[0190] Solvent Blue 36 (Nanjing Kangmanlin Chemical Industry) 5.5 parts

[0191] Silicone oil (KM-244F Shin-Etsu silicone) 0.05 parts

[0192] 2-Butanone 44.5 parts

[0193] Toluene 44.5 parts

[0194] The coating was performed using a gravure coater with a coating thickness of 1.0 μm.

[0195] Sublimation ribbon comparison example 2:

[0196] The adhesive layer and back coating are consistent with Example 1, and the dye layer formula is as follows:

[0197] yellow:

[0198] Polyurethane (901H Wanhua Chemical) 4.5 parts

[0199] Solvent Yellow 2 (Henan Wokas Biotechnology) 5.5 parts

[0200] 2-Butanone 44.5 parts

[0201] Toluene 44.5 parts

[0202] Magenta:

[0203] Polyurethane (901H Wanhua Chemical) 4.5 parts

[0204] Solvent Red 24 (Sinopharm Chemical Reagent) 5.5 parts

[0205] 2-Butanone 44.5 parts

[0206] Toluene 44.5 parts

[0207] blue:

[0208] Polyurethane (901H Wanhua Chemical) 4.5 parts

[0209] Solvent Blue 36 (Nanjing Kangmanlin Chemical Industry) 5.5 parts

[0210] 2-Butanone 44.5 parts

[0211] Toluene 44.5 parts

[0212] The coating was performed using a gravure coater with a coating thickness of 1.0 μm.

[0213] Sublimation ribbon comparison example 3:

[0214] The dye layer and the back coating are consistent with those in Comparative Example 1, and the adhesive layer formula is as follows:

[0215] Polyvinyl pyrrolidone (industrial grade PVP K90 Guangdong Yuemei Chemical) 2 parts

[0216] Polyvinyl alcohol (Tianjin Damao Chemical) 2 parts

[0217] 48 parts water

[0218] 48 parts of isopropyl alcohol

[0219] Coating thickness 0.2μm.

[0220] Sublimation ribbon comparison example 4:

[0221] The dye layer and the bonding layer are consistent with those in Comparative Example 2, and the back coating formula is as follows:

[0222] 3 parts of polyvinyl butyral (B265H-B Guangzhou Hongshang)

[0223] Cellulose acetate butyrate (CAB393-3 American Eastman) 7 parts

[0224] Isocyanate ( Wanhua Chemical) 5 copies

[0225] Silicone oil (KF-6001 Shin-Etsu silicone) 0.2 parts

[0226] 2-Butanone 59.5 parts

[0227] Toluene 25.5 parts

[0228] Coating thickness 0.6μm.

[0229] Sublimation ribbon comparison example 5:

[0230] The dye layer and the bonding layer are consistent with those in Comparative Example 2, and the back coating formula is as follows:

[0231] 3 parts of polyvinyl butyral (B265H-B Guangzhou Hongshang)

[0232] Cellulose acetate butyrate (CAB393-3 American Eastman) 7 parts

[0233] Isocyanate ( Wanhua Chemical) 5 copies

[0234] Zinc stearate (Henan Xinzhiyuan Chemical) 0.3 parts

[0235] 2-Butanone 58 parts

[0236] Toluene 25.4 parts

[0237] Coating thickness 0.6μm.

[0238] Substrate coating example 1:

[0239] The substrate is a 50μm thick PET film, and the manufacturer is Dongguan Shunming Electronic Materials.

[0240] <Base coating>:

[0241] Polyurethane (905H Wanhua Chemical) 20 parts

[0242] Anti-hydrolysis agent (AS4 German Rhein Chemie) 0.5 parts

[0243] Isocyanate ( Wanhua Chemical) 0.5 parts

[0244] 2-Butanone 39.5 parts

[0245] Toluene 39.5 parts

[0246] The coating was carried out by a gravure coater, and the coating thickness was 1.5 μm.

[0247] <Printing layer>:

[0248] Vinyl chloride-vinyl acetate copolymer (MLC-14-55 Pangao Chemical) 20 parts

[0249] Silicone resin (KF-6123 Shin-Etsu silicone) 0.5 parts

[0250] Isocyanate ( Wanhua Chemical) 0.5 parts

[0251] 2-Butanone 39.5 parts

[0252] Toluene 39.5 parts

[0253] Coating was done by gravure coater, with a coating thickness of 5 μm.

[0254] Substrate coating example 2:

[0255] The substrate is a 75μm thick matte BOPP film, and the manufacturer is Zhongshan Xinguan Adhesive Products.

[0256] <Base coating>:

[0257] CPP treatment agent (YL-26GN2 Hangzhou Yunli Technology) 10 copies

[0258] Polyester resin (VYLON-200, Toyobo, Japan) 10 parts

[0259] 2-Butanone 39.5 parts

[0260] Toluene 39.5 parts

[0261] Coating was done by gravure coater, with a coating thickness of 1.5 μm.

[0262] The substrate layer is consistent with substrate coating example 1.

[0263] Substrate coating example 3:

[0264] The substrate is 75μm thick coated paper, and the manufacturer is Japan Prince Paper.

[0265] <Base coating>:

[0266] Polyurethane (905H Wanhua Chemical) 10 parts

[0267] 5 parts of polyurethane foam (2040M Changxing Chemical Industry)

[0268] Titanium dioxide (BLR-699 Hebei Bangti) 8 parts

[0269] Fluorescent brightener (LR-B Henan Longrui Chemical) 0.2 parts

[0270] 2-Butanone 38.4 parts

[0271] Toluene 38.4 parts

[0272] Coating was done by gravure coater, with a coating thickness of 4 μm.

[0273] The substrate layer is consistent with substrate coating example 1.

[0274] Substrate coating comparison example 1:

[0275] The substrate is a 50μm thick PET film, and the manufacturer is Dongguan Shunming Electronic Materials.

[0276] There is no primer layer, and the substrate layer is consistent with substrate coating example 1.

[0277] Substrate coating comparison example 2:

[0278] The substrate is a 75μm thick matte BOPP film, and the manufacturer is Zhongshan Xinguan Adhesive Products.

[0279] There is no primer layer, and the substrate layer is consistent with substrate coating example 1.

[0280] Substrate coating comparison example 3:

[0281] The substrate is 75μm thick coated paper, and the manufacturer is Japan Prince Paper.

[0282] There is no primer layer, and the substrate layer is consistent with substrate coating example 1.

[0283] Performance test plan:

[0284] The printing test was carried out using a Hunan Dingyiyuan DT-330A sublimation soft label printer with a printing speed of 6m / min. The test pattern was a 255 grayscale image. The color density test was carried out using an X-Rite i1-PRO3 colorimeter. The printing ribbon was the YMC tricolor ribbon of sublimation ribbon examples 1-8 and sublimation ribbon comparison examples 1-5. The printing substrate was substrate coating examples 1-3 and substrate coating comparison examples 1-3. The test results after continuous printing for 1000m are as follows:

[0285]

[0286] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A thermal sublimation ribbon that maintains high color density under high-speed printing, characterized in that: The invention comprises a back coating layer, a substrate, a bonding layer and a dye layer which are arranged in sequence, wherein the dye layer comprises at least a dye, a resin, an organic silicone oil and a solvent, the weight ratio of the dye to the resin is (1:0.8)-(1:0.6), and the content of the organic silicone oil is 0.1-5 phr of the resin; The dye is a solvent-based thermal sublimation dye; The resin is polyurethane; The organic silicone oil is a non-reactive organic silicone oil; The solvent is a mixed reagent of butanone and toluene, and its content is greater than or equal to 89 phr of the dye layer; The total thickness of the dye layer is 0.5-1.5 μm; The dye layer also includes an isocyanate curing agent, the content of which is 1-10 phr of the resin; The material of the bonding layer includes any one or more of polyvinyl pyrrolidone, polyvinyl alcohol, polyvinyl acetal, polyvinyl butyral, and methyl cellulose; the thickness of the bonding layer is 0.1-0.5 μm.

2. The thermal sublimation ribbon for maintaining high color density under high-speed printing according to claim 1, characterized in that: The dye layer also includes a solid lubricant, the content of which is 0.5-1.5 phr of the resin.

3. The thermal sublimation ribbon for maintaining high color density under high-speed printing according to claim 1, characterized in that: The base material is a PET film; The thickness of the substrate is 4-125 μm.

4. The thermal sublimation ribbon for maintaining high color density under high-speed printing according to claim 1, characterized in that: In the back coating: The heat-resistant resin comprises one or more selected from polyvinyl butyral resin, polyvinyl acetal resin, polyester resin, polyurethane resin, polycarbonate resin and cellulose acetate butyrate; Including 0.5-5phr of heat-resistant resin silicone oil; The invention comprises 0.5-10 phr of a heat-resistant resin as a solid lubricant, wherein the solid lubricant is selected from one or more of phosphate ester, zinc stearate, organic silicon resin particles or talc.