An electron transport material and its preparation method and application
By designing the electron transport material of polycyclic aromatic hydrocarbon compounds containing unsaturated bonds, the problems of poor thermal stability and low transmission efficiency in OLED devices are solved, and efficient charge transfer and long-life OLED device performance is achieved, reducing the driving voltage.
Patent Information
- Application Number
- CN202110812404.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-07-19
AI Technical Summary
Existing electronic transmission materials have problems in OLED devices with poor thermal stability, low transmission efficiency and crystallization affecting the life of the device, and cannot meet the needs of low driving voltage, high efficiency, high brightness and long life.
An electron transport material containing unsaturated bonds is designed to improve the charge transfer capability and thermal stability of electron transport materials through the synergistic effect of specific parent core structure and conjugated substituents. It is used for electrons in OLED devices. Transport layer.
It improves the luminous performance and service life of OLED devices, reduces the driving voltage, the current efficiency reaches 7.35~8.75Cd/A, the T95 reaches 258~280h, and the driving voltage is reduced to 3.53~3.59V.
Smart Images

Figure FDA0004971453360000011 
Figure FDA0004971453360000012 
Figure FDA0004971453360000021
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of organic photoelectric materials, and in particular to an electron transport material and a preparation method and application thereof. Background Art
[0002] Organic electroluminescence (EL) is the emission of light by organic materials stimulated by electrical energy. Organic light-emitting diode (OLED) is a device that uses a multi-layer organic thin film structure to produce electroluminescence. It is simple to prepare and only requires a very low driving voltage. Compared with LCD, it has excellent display characteristics and quality, such as self-luminescence, wide viewing angle, high efficiency, wide color gamut, and flexible display.
[0003] Select high-performance OLED functional materials and make reasonable combinations to give full play to the comprehensive characteristics of high efficiency, long life and low voltage of the device. The materials that constitute the organic material layer, such as hole transport materials, luminescent materials, electron transport materials, etc., should have the following characteristics: high efficiency fluorescence in the visible light region, high conductivity, good semiconductor properties; good film-forming properties, and the formed thin film has good uniformity, etc.
[0004] CN111548350A relates to the technical field of organic optoelectronic materials, and specifically discloses a polycyclic aromatic hydrocarbon naphthazoline derivative and a synthesis method thereof and an electronic device containing the polycyclic aromatic hydrocarbon naphthazoline derivative. The polycyclic aromatic hydrocarbon naphthazoline derivative disclosed herein has excellent film-forming property and thermal stability by introducing a polycyclic aromatic hydrocarbon naphthazoline rigid structure, and can be used to prepare organic electroluminescent devices, organic field effect transistors and organic solar cells. In addition, the polycyclic aromatic hydrocarbon naphthazoline derivative disclosed herein can be used as a constituent material of a hole injection layer, a hole transport layer, a light-emitting layer, an electron blocking layer, a hole blocking layer or an electron transport layer, and can reduce the driving voltage, improve efficiency, brightness and life, etc.
[0005] CN103811657A discloses an organic photovoltaic cell with an electron transport layer and a hole transport layer, comprising a substrate, an anode, a hole transport layer, an active layer, an electron transport layer and a cathode stacked in sequence, wherein the active layer comprises a stacked electron donor material and an electron acceptor material, wherein the electron acceptor material is carbon 60 and its derivatives or carbon 70 and its derivatives; the cell has a high energy conversion efficiency.
[0006] Although electron transport materials and their applications in OLED devices have been disclosed in the prior art, there are still relatively few types of electron transport materials, and there are also problems such as poor thermal stability, low transport efficiency, and crystallization during use that affects the life of the device, which cannot meet the device's preparation process requirements and performance requirements.
[0007] In summary, developing more types of electron transport materials with excellent stability and high-efficiency transport performance to meet the needs of low driving voltage, high efficiency, high brightness and long life of OLEDs is the research focus in this field. Summary of the invention
[0008] In view of the deficiencies in the prior art, the purpose of the present invention is to provide an electron transport material and a preparation method and application thereof. By designing the parent core structure of the compound and introducing substituents at specific sites, the electron transport material is endowed with excellent charge transfer ability and good thermal stability. As an electron transport material for an electroluminescent device, it can effectively improve the luminescence performance and service life of the device.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides an electron transport material having a structure as shown in Formula I:
[0011]
[0012] Wherein, L is selected from any one of a single bond, a substituted or unsubstituted C6-C60 arylene group, a substituted or unsubstituted C3-C60 cycloalkyl group, and a substituted or unsubstituted C2-C60 heterocyclic group;
[0013] Ar is at least one selected from a substituted or unsubstituted C6-C60 aryl group, a substituted or unsubstituted C2-C60 heterocyclic group, and a substituted or unsubstituted C3-C60 cycloalkyl group.
[0014] The "C6-C60" mentioned in the present invention refers to the number of carbon atoms in the group, and the same applies to "C3-C60" and "C2-C60".
[0015] The C6~C60 can be C6, C7, C8, C9, C10, C12, C15, C18, C20, C22, C24, C25, C27, C29, C32, C35, C38, C40, C42, C45, C48, C50, C52, C55, C57, C59, etc.
[0016] The C3~C60 can be C4, C5, C6, C8, C10, C12, C15, C18, C20, C22, C24, C25, C27, C29, C32, C35, C38, C40, C42, C45, C48, C50, C52, C55, C57, C59, etc.
[0017] The C2~C60 can be C3, C4, C5, C6, C8, C10, C12, C15, C18, C20, C22, C24, C25, C27, C29, C32, C35, C38, C40, C42, C45, C48, C50, C52, C55, C57, C59, etc.
[0018] The electron transport material provided by the present invention is a class of polycyclic aromatic hydrocarbon compounds containing unsaturated bonds. The mother core structure of the specific structure makes the electron transport material have a large conjugation effect. The substituents with conjugation effect synergistically act with the mother core structure to further enhance the conjugation effect of the electron transport material, so that the electron transport material has excellent electron transport ability, thereby effectively improving the luminescence performance and service life of the device and reducing the driving voltage.
[0019] Preferably, the heteroatom in the heterocyclic group is selected from any one of O, N, S or Si.
[0020] In the present invention, the arylene group illustratively includes, but is not limited to, phenylene, biphenylene, terphenylene, naphthylene, anthrylene, phenanthrylene or fluorenylene.
[0021] The aryl group includes, but is not limited to, phenyl, biphenyl, terphenyl, naphthyl, anthracenyl, phenanthrenyl, pyrenyl, perylenyl, fluorenyl or spirofluorenyl, etc.
[0022] The heteroaryl group includes, but is not limited to, N-phenylcarbazolyl, furanyl, thienyl, pyrrolyl, pyridyl, pyrazinyl, pyrimidinyl, pyridazinyl, triazine, carbazolyl, acridinyl, imidazolyl, oxazolyl, thiazolyl, indolyl, benzofuranyl, benzothienyl, dibenzofuranyl, dibenzothienyl, benzimidazolyl, quinolyl or isoquinolyl, etc.
[0023] Preferably, the arylene group is selected from any one of phenylene, biphenylene, terphenylene, naphthylene, anthracene, phenanthrylene or fluorenylene.
[0024] Preferably, the aryl group is selected from any one of phenyl, biphenyl, terphenyl, naphthyl, anthracenyl, phenanthrenyl, pyrenyl, perylenyl, fluorenyl or spirofluorenyl.
[0025] Preferably, the heteroaryl group is selected from any one of N-phenylcarbazolyl, furanyl, thienyl, pyrrolyl, pyridyl, pyrazinyl, pyrimidinyl, pyridazinyl, triazine, carbazolyl, acridinyl, imidazolyl, oxazolyl, thiazolyl, indolyl, benzofuranyl, benzothienyl, dibenzofuranyl, dibenzothienyl, benzimidazolyl, quinolyl or isoquinolyl.
[0026] Preferably, L is selected from triazine groups.
[0027] The reason why L in the present invention is preferably a triazine group is that the triazine group has a strong electron-withdrawing ability.
[0028] Preferably, Ar is selected from at least one of the following groups:
[0029]
[0030] Wherein, “—” represents the connecting bond of the group.
[0031] Preferably, the electron transport material comprises any one or a combination of at least two of the following compounds H1-H15:
[0032]
[0033]
[0034]
[0035] In a second aspect, the present invention provides a method for preparing the electron transport material according to the first aspect, the preparation method comprising: and Carrying out a coupling reaction under the action of a catalyst to obtain the electron transport material;
[0036] L and Ar each independently have the same defined range as above;
[0037] The X is a halogen.
[0038] Preferably, the catalyst is a palladium catalyst. Preferably, X is Cl.
[0039] In a third aspect, the present invention provides an OLED device, which comprises at least an anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer and a cathode stacked in sequence, and the material of the electron transport layer comprises the electron transport material described in the first aspect.
[0040] Preferably, the thickness of the hole injection layer is 55-65 nm, for example, 56 nm, 57 nm, 58 nm, 59 nm, 60 nm, 61 nm, 62 nm, 63 nm, 64 nm, etc.
[0041] Preferably, the thickness of the hole transport layer is 75-85 nm, for example, 76 nm, 77 nm, 78 nm, 79 nm, 80 nm, 81 nm, 82 nm, 83 nm, 84 nm, etc.
[0042] Preferably, the thickness of the light-emitting layer is 25-35 nm, for example, 26 nm, 27 nm, 28 nm, 29 nm, 30 nm, 31 nm, 32 nm, 33 nm, 34 nm, etc.
[0043] Preferably, the thickness of the electron transport layer is 35-45 nm, for example, 36 nm, 37 nm, 38 nm, 39 nm, 40 nm, 41 nm, 42 nm, 43 nm, 44 nm, etc.
[0044] Preferably, the thickness of the electron injection layer is 1-3 nm, for example, 1.2 nm, 1.4 nm, 1.6 nm, 1.8 nm, 2 nm, 2.2 nm, 2.4 nm, 2.6 nm, 2.8 nm, etc.
[0045] In a fourth aspect, the present invention provides an electronic device, comprising the OLED device described in the third aspect.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] The electron transport material of the present invention has excellent charge transfer ability and good thermal stability. As an electron transport material of an electroluminescent device, it can effectively improve the luminescence performance and service life of the device, with a current efficiency of 7.35-8.75Cd / A, a T95 of 258-280h, and a driving voltage reduced to 3.53-3.59V. DETAILED DESCRIPTION
[0048] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0049] The compound raw materials in the following examples of the present invention (including compounds A1-A9) can all be purchased from the market.
[0050] Example 1
[0051] This embodiment provides an electron transport material having the following structure:
[0052]
[0053] The preparation method is as follows:
[0054]
[0055] Under argon atmosphere, 3 g of intermediate A1, 4 g of intermediate A2, 0.16 mmol of palladium acetate (Pd(pph) 3 ) 4), 0.32 mmol of tri-tert-butylphosphine, 9.6 mmol of potassium carbonate (K 2 CO 3 ) and 50 mL of tetrahydrofuran (THF), stirred at 125° C. for 12 h, and the solid obtained by the reaction was separated by silica gel column chromatography and purified by recrystallization to obtain 4.3 g of the target product compound H1 with a yield of 61%.
[0056] The target product structure was tested by mass spectrometry (HRMS):
[0057] C 51 H 33 N 3 O, calculated molecular weight: 703.26, tested value: 703.84;
[0058] Elemental analysis theoretical values: C: 87.03, O: 2.27, N: 5.97, H: 4.73;
[0059] Elemental analysis test values: C: 87.23, O: 2.47, N: 5.97, H: 4.55.
[0060] Example 2
[0061] This embodiment provides an electron transport material having the following structure:
[0062]
[0063] The preparation method is as follows:
[0064]
[0065] Under an argon atmosphere, 3 g of intermediate A3, 4 g of intermediate A2, 0.16 mmol of palladium acetate, 0.32 mmol of tri-tert-butylphosphine, 9.6 mmol of potassium carbonate and 50 mL of tetrahydrofuran were stirred at 125°C for 12 h. The solid obtained by the reaction was separated by silica gel column chromatography and purified by recrystallization to obtain 5.1 g of the target product compound H2 with a yield of 66%.
[0066] The target product structure was tested by mass spectrometry (HRMS):
[0067] C 64 H 43 N 3 , calculated molecular weight: 853.35, tested value: 854.07;
[0068] Elemental analysis theoretical values: C: 90.00, N: 4.92, H: 5.07;
[0069] Elemental analysis test values: C: 90.02, N: 4.91, H: 5.09.
[0070] Example 3
[0071] This embodiment provides an electron transport material having the following structure:
[0072]
[0073] The preparation method is as follows:
[0074]
[0075] Under an argon atmosphere, 2 g of intermediate A4, 4 g of intermediate A2, 0.16 mmol of palladium acetate, 0.32 mmol of tri-tert-butylphosphine, 9.6 mmol of potassium carbonate and 50 mL of tetrahydrofuran were mixed and stirred at 125°C for 12 h. The solid obtained by the reaction was separated by silica gel column chromatography and purified by recrystallization to obtain 4.2 g of the target product compound H3 with a yield of 66%.
[0076] The target product structure was tested by mass spectrometry (HRMS):
[0077] C 57 H 39 N 3 , calculated molecular weight: 765.31, tested value: 765.96;
[0078] Elemental analysis theoretical values: C: 89.38, N: 5.49, H: 5.07;
[0079] Elemental analysis test values: C: 89.48, N: 5.45, H: 5.13.
[0080] Example 4
[0081] This embodiment provides an electron transport material having the following structure:
[0082]
[0083] The preparation method is as follows:
[0084]
[0085] Under an argon atmosphere, 3 g of intermediate A5, 4 g of intermediate A6, 0.16 mmol of palladium acetate, 0.32 mmol of tri-tert-butylphosphine, 9.6 mmol of potassium carbonate and 50 mL of tetrahydrofuran were mixed and stirred at 125°C for 12 h. The solid obtained by the reaction was separated by silica gel column chromatography and purified by recrystallization to obtain 4.0 g of the target product compound H4 with a yield of 62%.
[0086] The target product structure was tested by mass spectrometry (HRMS):
[0087] C 51 H 33 N 3 S, calculated molecular weight: 719.24, tested value: 719.24;
[0088] Elemental analysis theoretical values: C: 85.09, S: 4.45, N: 5.84, H: 4.62;
[0089] Elemental analysis test values: C: 85.13, S: 4.42, N: 5.81, H: 4.60.
[0090] Example 5
[0091] This embodiment provides an electron transport material having the following structure:
[0092]
[0093] The preparation method is as follows:
[0094]
[0095] Under an argon atmosphere, 3 g of intermediate A7, 4 g of intermediate A6, 0.16 mmol of palladium acetate, 0.32 mmol of tri-tert-butylphosphine, 9.6 mmol of potassium carbonate and 50 mL of tetrahydrofuran were mixed and stirred at 125°C for 12 h. The solid obtained by the reaction was separated by silica gel column chromatography and purified by recrystallization to obtain 3.9 g of the target product compound H5 with a yield of 60%.
[0096] The target product structure was tested by mass spectrometry (HRMS):
[0097] C 50 H 34 N 4 , calculated value: 690.28, tested value: 690.85;
[0098] Elemental analysis theoretical values: C: 86.93, N: 8.11, H: 4.96;
[0099] Elemental analysis test values: C: 86.95, N: 8.14,; H: 4.92.
[0100] Example 6
[0101] This embodiment provides an electron transport material having the following structure:
[0102]
[0103] The preparation method is as follows:
[0104]
[0105] Under an argon atmosphere, 3 g of intermediate A8, 4 g of intermediate A6, 0.16 mmol of palladium acetate, 0.32 mmol of tri-tert-butylphosphine, 9.6 mmol of potassium carbonate and 50 mL of tetrahydrofuran were mixed and stirred at 125°C for 12 h. The solid obtained by the reaction was separated by silica gel column chromatography and purified by recrystallization to obtain 4.0 g of white solid H6 with a yield of 62%.
[0106] The target product structure was tested by mass spectrometry (HRMS):
[0107] C 50 H 34 N 4 , calculated value: 690.28, tested value: 690.85;
[0108] Elemental analysis theoretical values: C: 86.93, N: 8.11, H: 4.96;
[0109] Elemental analysis test values: C: 86.95, N: 8.14,; H: 4.92.
[0110] Application Example 1
[0111] An OLED device, comprising an anode, a hole injection layer, a hole transport layer, a light emitting layer, an electron transport layer, an electron injection layer and a cathode stacked in sequence; the material composition of each layer is as follows:
[0112] Anode: 60nm thick, indium tin oxide (ITO);
[0113] Hole injection layer: thickness 60nm, HIL;
[0114] Hole transport layer: thickness 80nm, HTL;
[0115] Light-emitting layer: Thickness is 30nm, main material is BH 3 , the dopant is BD, and the mass ratio of the two is 95:1;
[0116] Electron transport layer: 40 nm thick, the electron transport material provided in Example 1 of the present invention (Compound H1);
[0117] Electron injection layer: 2nm thick, LiF;
[0118] Cathode: 150nm thick, aluminum.
[0119] The hole injection layer, hole transport layer, light emitting layer, electron transport layer, electron injection layer and cathode of the OLED device are prepared by vacuum deposition.
[0120]
[0121]
[0122] Application Example 2
[0123] An OLED device, which is different from Application Example 1 only in that the compound H1 in the electron transport layer is replaced by the electron transport material (compound H2) provided in Example 2 of the present invention.
[0124] Application Example 3
[0125] An OLED device, which is different from Application Example 1 only in that the compound H1 in the electron transport layer is replaced by the electron transport material (compound H3) provided in Example 3 of the present invention.
[0126] Application Example 4
[0127] An OLED device, which is different from Application Example 1 only in that the compound H1 in the electron transport layer is replaced by the electron transport material (compound H4) provided in Example 4 of the present invention.
[0128] Application Example 5
[0129] An OLED device, which is different from Application Example 1 only in that the compound H1 in the electron transport layer is replaced by the electron transport material (compound H5) provided in Example 5 of the present invention.
[0130] Application Example 6
[0131] An OLED device, which differs from Application Example 1 only in that the compound H1 in the electron transport layer is replaced by the electron transport material (compound H6) provided in Example 6 of the present invention.
[0132] Application Comparative Example 1
[0133] An OLED device, which differs from Application Example 1 only in that the compound H1 in the electron transport layer is replaced by the electron transport material (compound D1) provided in Example 1 of the present invention, and has the following structural formula:
[0134]
[0135] Application Comparative Example 2
[0136] An OLED device, which differs from Application Example 1 only in that the compound H1 in the electron transport layer is replaced by the electron transport material (compound D2) provided in Example 1 of the present invention, and has the following structural formula:
[0137]
[0138] The preparation method of D2 is different from that of Example 1 in that A1 is replaced by A9
[0139] The target product structure was tested by mass spectrometry (HRMS):
[0140] C 33 H 23 N 3 , calculated molecular weight: 461.19, tested value: 461.57;
[0141] Elemental analysis theoretical values: C: 85.87, N: 9.10, H: 5.02;
[0142] Elemental analysis test values: C: 85.67, N: 9.22, H: 5.06.
[0143] Performance test of OLED devices:
[0144] The OLED devices provided in Application Examples 1-6 and Comparative Examples 1-2 were tested for luminous efficiency, and the electroluminescent spectra and current-voltage-luminous density characteristics (IUL characteristics) were measured. 2 The electroluminescence spectrum is measured at a luminous density of 1.5 %. The lifespan TL1 is defined as the time it takes for the brightness to drop from the initial brightness to a specific proportion L1 during operation at a constant current. Therefore, T95 is the time it takes for the brightness to drop to 95% of its initial value during operation. In the above test, 40 mA / cm 2 The current density was taken as the operating condition.
[0145] The performance test results are shown in Table 1:
[0146] Table 1
[0147]
[0148]
[0149] According to the data in Table 1, the electron transport material provided by the present invention is suitable for use as an electron transport layer material in an OLED device. The OLED device using the electron transport material of the present invention as an electron transport layer has a current efficiency of 7.35 to 8.75 Cd / A, a T95 of 258 to 280 h, and a driving voltage reduced to 3.53 to 3.59 V, which effectively improves the luminous efficiency of the device, prolongs the service life of the device, and reduces the driving voltage.
[0150] In the charge transport material provided by the present invention, a specific core structure and a plurality of substituents cooperate with each other, so that the charge transport material has excellent charge transfer ability. Changes in the core structure (application comparison example 1) or the absence of substituents (application comparison example 2) will lead to a decrease in the material's transfer efficiency and affect the performance of the device.
[0151] The present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. An OLED device, It is characterized in that The OLED device comprises an anode, a hole injection layer, a hole transport layer, a light emitting layer, an electron transport layer, an electron injection layer and a cathode which are stacked in sequence, and the material of the electron transport layer comprises an electron transport material; The material of the hole injection layer is: The material of the hole transport layer is: The electron transport material is:
2. The OLED device according to claim 1, It is characterized in that The preparation method of the electron transport material comprises the following steps: and Carrying out a coupling reaction under the action of a catalyst to obtain the electron transport material; The L is a triazine group; The Ar is The X is a halogen.
3. The OLED device according to claim 2, It is characterized in that The catalyst is a palladium catalyst.
4. The OLED device according to claim 2, It is characterized in that The X is Cl.
5. The OLED device according to claim 1, It is characterized in that The thickness of the hole injection layer is 55-65 nm.
6. The OLED device according to claim 1, It is characterized in that The thickness of the hole transport layer is 75-85 nm.
7. The OLED device according to claim 1, It is characterized in that The thickness of the light-emitting layer is 25-35 nm.
8. The OLED device according to claim 1, It is characterized in that The thickness of the electron transport layer is 35-45 nm.
9. The OLED device according to claim 1, It is characterized in that The thickness of the electron injection layer is 1-3 nm.