A method for preparing a tantalum-tantalum carbide composite coating and its products
The preparation of tantalum-tantalum carbide composite coating on the surface of the substrate by chemical vapor deposition method solves the problems of poor ductility and high processing cost of tantalum carbide materials, achieves a high-purity, dense pore-free coating, reduces production costs, and Improves the high temperature resistance and chemical stability of the coating.
Patent Information
- Application Number
- CN202211247928.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-10-12
AI Technical Summary
Tantalum carbide ceramic materials are difficult to widely use due to poor ductility, fragility and high processing costs. In addition, chemical vapor deposition methods have problems of low efficiency and poor adhesion when preparing tantalum-tantalum carbide coatings.
The tantalum-tantalum carbide composite coating is prepared on the surface of the substrate by chemical vapor deposition method, and the tantalum carbide coating is deposited through heating steps, combining tantalum pentachloride or tantalum pentafluoride gas, hydrogen and mixed olefins and other gases. Control the reaction temperature and air pressure to form a high-purity, dense, poreless tantalum-tantalum carbide composite coating.
It realizes the high purity, strong binding force, high temperature resistance and chemical stability of the tantalum-tantalum carbide composite coating, reduces production costs, is suitable for industrial large-scale production, and effectively protects the substrate, and is suitable for the surface of various high-temperature materials.
Smart Images

Figure CN115637419B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal-ceramic composite materials, and particularly relates to a preparation method of a tantalum-tantalum carbide composite coating and a product thereof. Background Art
[0002] Tantalum carbide ceramics are a kind of ceramic material with superconductivity, golden appearance, high hardness (2100HV0.05), high melting point (3880℃), corrosion resistance, and non-sticking advantages. It is an emerging ceramic material in recent years. Powdered tantalum carbide is widely used in the smelting process of special alloys. Tantalum carbide ceramics have broad application prospects in semiconductors, chemical industry, metallurgy, mold processing, aerospace and other fields. It is an excellent shielding and wear-resistant material. However, its poor ductility, fragility, and high processing costs restrict its widespread use.
[0003] Chemical vapor deposition (CVD) is a complex process that includes the thermodynamics and kinetics of chemical reactions as well as heat transfer, mass transfer and other effects. On the one hand, the chemical reaction must be controlled to occur in the reaction chamber, and on the other hand, the product must form a crystal nucleus on the surface of the blank and grow. In other words, there is a possibility of chemical reaction between chemical substances, but there is no guarantee that the reaction process will occur efficiently. After many experiments, the process parameters are continuously optimized.
[0004] Tantalum carbide materials are generally difficult to process and shape using machining processes due to their high melting point, high hardness, and poor ductility. The commonly used hot pressing and sintering method is difficult to achieve dense and pore-free. Tantalum carbide materials may have poor adhesion on the surface of some substrates due to their high hardness and poor ductility; therefore, the preparation of tantalum-tantalum carbide coating products by chemical vapor deposition (CVD) has great significance and broad application prospects.
[0005] The composite coating is mainly used to improve the bonding strength and density of the product, especially between two layers of materials with large differences in thermal expansion coefficients. The metal layer can be used as a buffer layer. The toughness and density of the metal are better than those of ceramic materials, which can effectively reduce the porosity of the coating. Summary of the invention
[0006] The present invention aims at the shortcomings of existing tantalum carbide coated products, uses a chemical vapor deposition method to prepare a tantalum-tantalum carbide composite coating on the surface of a substrate, and provides a method for preparing a tantalum-tantalum carbide coated product with corrosion resistance, wear resistance, good appearance quality, and low adhesion.
[0007] In order to achieve the above-mentioned purpose, the solution of the present invention is: a product of tantalum-tantalum carbide composite coating, including a substrate, and a tantalum-tantalum carbide coating formed on the surface of the substrate, the substrate includes a metal material, and is also suitable for high-temperature resistant materials such as carbon materials, ceramic materials and quartz materials.
[0008] The present invention also provides a method for preparing a tantalum-tantalum carbide composite coating, which specifically comprises the following steps:
[0009] ① Heating step: placing the substrate in a reaction chamber, evacuating the reaction chamber, and heating the reaction chamber, wherein the heating temperature is 800-1100° C.;
[0010] ② Tantalum coating deposition step: After the heating step, tantalum pentachloride or tantalum pentafluoride gas and hydrogen are introduced into the reaction chamber, and the reaction temperature is maintained at 800~1100°C under a pressure of 3000Pa to 6000Pa to deposit a tantalum coating on the surface of the substrate;
[0011] ③ Cooling step: stop introducing the reaction gas, cool down, and start keeping warm when the temperature drops to 550~750℃;
[0012] ④ Tantalum carbide coating deposition step: introduce tantalum pentachloride or tantalum pentafluoride gas, mixed olefins and hydrogen mixed gas into the reaction chamber, maintain the reaction temperature at 550-750°C under a pressure of 5000Pa to 10000Pa, and deposit a tantalum carbide coating on the surface of the substrate to obtain a tantalum-tantalum carbide composite coating material;
[0013] ⑤ Cooling step: After the above steps, the tantalum-tantalum carbide coated product is cooled to room temperature;
[0014] ⑥Cleaning step: After cooling to room temperature, take out the product and clean it with deionized water and ethanol respectively.
[0015] Furthermore, the gasification temperature of the tantalum pentachloride or tantalum pentafluoride is 300-500°C.
[0016] Preferably, the reaction chamber is a stainless steel reaction chamber.
[0017] Preferably, the mixed olefins are a mixture of ethylene and propylene; the volume ratio of ethylene to propylene is 1:1-2.
[0018] Furthermore, the volume ratio of tantalum pentachloride or tantalum pentafluoride gas to hydrogen in step ② or step ④ is 1:1-2.5.
[0019] Furthermore, in step ④, the volume ratio of tantalum pentachloride or tantalum pentafluoride gas to mixed olefins is 1:1-2.
[0020] Preferably, in step ②, the tantalum pentachloride or tantalum pentafluoride gas can be introduced into the reaction chamber by a carrier gas, and the carrier gas is argon; the volume ratio of the tantalum pentachloride or tantalum pentafluoride gas to the carrier gas is 1:1~3.
[0021] Preferably, the flow rate of the tantalum pentachloride or tantalum pentafluoride gas is 2-6 SLM, the flow rate of the mixed olefin gas is 2-12 SLM, the flow rate of the argon gas is 1-6 SLM, and the flow rate of the hydrogen gas is 2-15 SLM.
[0022] After adopting the above scheme, the beneficial effect achieved is: the present invention uses tantalum halide, hydrogen and olefin as raw materials, and produces high-purity tantalum-tantalum carbide composite coating materials through chemical vapor deposition, which effectively solves the drawbacks of existing tantalum carbide coating products and reduces production costs, and is suitable for industrial-scale production.
[0023] (1) The tantalum-tantalum carbide composite coating prepared by this method has high purity and is free of impurities.
[0024] (2) The tantalum coating in the tantalum-tantalum carbide composite coating prepared by the present invention has high bonding strength with the substrate and is free of pores.
[0025] (3) The tantalum carbide coating in the tantalum-tantalum carbide composite coating prepared by the present invention is resistant to high temperatures and has stable chemical properties and is not easy to react chemically with other substances.
[0026] (4) The tantalum-tantalum carbide composite coating prepared by the present invention combines the advantages of tantalum coating and tantalum carbide coating, effectively isolates the substrate from the external environment, and can effectively protect the substrate.
[0027] (5) A corrosion-resistant and wear-resistant tantalum-tantalum carbide isolation coating is prepared on the surface of the substrate by chemical vapor deposition. The thickness of the coating can be adjusted according to the actual product needs and can reach the millimeter level. This also shows that the coating product prepared by the present invention has strong bonding strength.
[0028] (6) The preparation method of the present invention has relatively loose requirements on the material of the substrate, because the substrate itself does not participate in the chemical reaction. In addition to carbon materials (graphite, carbon / carbon, etc.), the coating can also be deposited on the surface of high-temperature resistant materials such as corundum, high-temperature alloys, quartz, etc.; there is no requirement for the shape of the substrate, and it can be deposited on various special-shaped surfaces with good uniformity and dense structure.
[0029] (7) The present invention uses ethylene and propylene mixed olefins as one of the reactants. Ethylene and propylene are not easy to decompose at the current reaction temperature, and the product microstructure and performance are better. Compared with alkanes or alkynes, the biggest advantage of mixed olefin gas is high efficiency and safety. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1This is a cross-sectional view of the composite coating of Example 1 (not polished);
[0031] Figure 2 is a cross-sectional view of the composite coating of Example 2;
[0032] Figure 3 is another cross-sectional view of the composite coating of Example 2;
[0033] Figure 4 This is a surface morphology of the tantalum carbide coating of Example 1;
[0034] Figure 5 This is a surface morphology of the tantalum carbide coating of Example 2;
[0035] Figure 6 This is a metallographic photograph of the tantalum carbide coating of Example 1;
[0036] Figure 7 This is a schematic diagram of the chemical vapor deposition equipment system structure used in the present invention. DETAILED DESCRIPTION
[0037] Tantalum carbide materials are generally difficult to process and shape using machining processes due to their high melting point, high hardness, and poor ductility. The commonly used hot pressing and sintering method is difficult to achieve dense and pore-free. Tantalum carbide materials may have poor adhesion on the surface of some substrates due to their high hardness and poor ductility; therefore, the preparation of tantalum-tantalum carbide coating products by chemical vapor deposition (CVD) has great significance and broad application prospects.
[0038] Tantalum halides provide a convenient inorganic source for the deposition of tantalum and tantalum carbide, especially tantalum pentahalide (TaX5), where X represents halogen fluorine (F) and chlorine (Cl). Table 1 shows the physical and chemical properties of tantalum halides tantalum pentafluoride (TaF5) and tantalum pentachloride (TaCl5). Tantalum pentafluoride and tantalum pentachloride are both solid at room temperature (18℃-22℃).
[0039] Table 1 Physical and chemical properties of tantalum pentahalide (TaX5) for deposition applications
[0040] Melting point(℃) Boiling point(℃) Change in heat of formation (ΔHf) <![CDATA[TaF5]]> 97 230 -455 kcal / mol <![CDATA[TaCl5]]> 216 242 -205 kcal / mol
[0041] The carbon source gas used in the traditional CVD process for depositing tantalum carbide is methane or propane. Alkanes have good stability and lower chemical reactivity than alkenes and alkynes. The reaction temperature of alkanes is high, side reactions will occur, and there are high requirements for equipment, and the reaction rate is also slow. Alkynes have the highest reactivity, the reaction temperature is very low, the coating deposition rate is also very fast, and they have extremely high production efficiency. The reaction temperature is low and the equipment requirements are also low. However, alkynes are prone to explosive cracking, which affects production safety. In addition, alkynes will undergo polymerization reactions, which have high quality requirements for control equipment and personnel.
[0042] The present invention adopts ethylene and propylene mixed olefins as one of the reactants. Ethylene and propylene are not easy to decompose at the current temperature, and the microstructure and performance of the product are better.
[0043] A method for preparing a tantalum-tantalum carbide composite coating product comprises the following steps:
[0044] (1) flushing and evacuating the vapor deposition equipment and all pipelines with an inert gas, wherein the inert gas is argon;
[0045] (2) Cleaning and decontaminating the green body to be deposited, drying it and placing it in a reaction chamber;
[0046] (3) Exhausting non-reactive gases and impurities that enter the vapor deposition equipment during the process of placing the green body;
[0047] (4) After checking that the vapor deposition equipment is sealed intact, the vacuum degree in the vapor deposition equipment is controlled to 3000-6000 Pa by a vacuum pump, and the temperature in the reaction chamber is heated to 800-1100° C.;
[0048] (5) placing tantalum pentachloride or tantalum pentafluoride in a vaporization chamber and heating it to 300-550° C. to vaporize it, and passing the vaporized tantalum pentachloride or tantalum pentafluoride gas into a gas mixing tank at a gas flow rate of 2-6 SLM. At the same time, passing hydrogen into the gas mixing tank at a hydrogen flow rate of 2-15 SLM. After the two gases are fully mixed in the gas mixing tank, they are passed into a reaction chamber to perform a chemical vapor deposition reaction on the blank, and heated for a certain period of time to deposit a tantalum coating on the surface of the substrate;
[0049] Stop introducing the reaction gas, cool down the temperature, and start keeping warm when the temperature drops to 550-750°C; introduce tantalum pentachloride or tantalum pentafluoride gas, mixed olefins and hydrogen mixed gas into the reaction chamber, keep the reaction temperature for a certain period of time at a pressure of 5000Pa to 10000Pa, and deposit a tantalum carbide coating on the surface of the substrate; obtain a tantalum-tantalum carbide composite coating material;
[0050] (6) Disconnect the heating power supply, stop heating, and allow the reaction chamber to cool down naturally; when the temperature in the reaction chamber drops below 60°C, turn off the vacuum pump and continue to introduce argon. After the reaction chamber is filled to normal pressure, stop introducing argon, open the exhaust valve, open the reaction chamber, and take out the prepared tantalum-tantalum carbide composite coating material. The thickness of the tantalum coating or tantalum carbide coating can be adjusted according to actual product needs.
[0051] Among them, the chemical vapor deposition equipment includes a vaporization chamber and a reaction chamber. Figure 1As shown, the chemical vapor deposition equipment 1 has a reaction chamber 11, and the deposition workpiece 12 (such as a blank) is placed in the reaction chamber 11. The reaction chamber 11 is provided with two vents, one of which is connected to the air inlet pipe 13, and the other is connected to the vacuum pipe 14. The reaction chamber 11 is also provided with a heating device (not shown in the figure) that can heat the reaction chamber, and the outer end of the vacuum pipe 14 is connected to the vacuum pump 17. The air inlet pipe 13 is connected to a mixing tank 16, and the mixing tank 16 is connected to at least one ventilation pipe 161. In this embodiment, two are provided to respectively introduce reducing gas and inert argon gas from the ventilation pipe 161. The mixing tank 16 is connected to a vaporization chamber 15, and the vaporization chamber 15 can heat and vaporize the initial tantalum halide. The vaporized tantalum halide gas enters the mixing tank 16 and is fully mixed with other gases. The flow rate of the reaction gas is adjusted by the gas control device 18.
[0052] In the vaporization chamber, solid reactants such as tantalum chloride or other tantalum halides are vaporized by heat energy to become gaseous. The gaseous reactants react in the reaction chamber to convert vapor such as tantalum halide into a tantalum deposit.
[0053] The reaction chamber for vapor deposition adopts a stainless steel reaction chamber. The stainless steel reaction chamber selected in the solution of the present invention has low cost and can ensure long-term stable operation, and is the best choice.
[0054] The purpose of steps (1) to (3) is to increase the bonding strength between the coating or composite material and the blank, and to perform pretreatment before chemical vapor deposition.
[0055] In step (4), the temperature of the reaction chamber needs to be high to ensure that the tantalum-chlorine bond or tantalum-fluorine bond in tantalum pentachloride or tantalum pentafluoride is completely dissociated, but the temperature of the reaction chamber should not be too high, otherwise the chemical deposition reaction will be carried out prematurely at other places before contacting the blank. The temperature affects the ionization degree of the reactants.
[0056] In step (5), the tantalum halide vapor is directly delivered to the reaction chamber by heating the solid tantalum halide to a temperature in the range of about 300 to 600° C., with the temperature selected depending on the specific reactants. The selected temperature must be sufficient to vaporize the reactants to provide a vapor pressure for delivering the tantalum halide vapor into the reaction chamber.
[0057] Tantalum carbide is prepared by using mixed olefin gas and tantalum pentachloride or tantalum pentafluoride gas. Compared with alkanes or alkynes, the biggest advantage of mixed olefin gas is high efficiency and safety. During the preparation process, the reaction temperature, vacuum degree, reaction gas flow rate and ratio have a major impact on the speed of the deposition reaction and the structure and performance of the deposited layer. The ratio of mixed olefin gas to tantalum halide gas and hydrogen affects the concentration of the reactants. Too low or too high a concentration of the reactants affects the deposition efficiency. The reaction gas must have enough residence time on the surface of the blank to participate in the reaction, and the deposition rate is controlled by the adsorption and desorption process between the reaction gas and the surface of the blank. When the gas flow rate increases, the source material participating in the reaction per unit time increases, which is conducive to the reaction in the direction of the product and the deposition rate increases. However, when the gas flow rate exceeds a certain range, some of the gas will not participate in the reaction and directly pass through the surface of the blank, causing waste. The process parameters in the chemical vapor deposition preparation process, such as reaction chamber temperature, equipment vacuum, reaction gas flow and ratio, tantalum halide vaporization temperature, deposition time and heat treatment process, all have an impact on the material properties of the product. They are mutually restrictive and complementary, and must be analyzed and adjusted in a unified manner when making process adjustments.
[0058] Preferably, the tantalum halide gas, mixed olefins and / or hydrogen are fully mixed in a gas mixing tank and then introduced into a reaction chamber for chemical vapor deposition reaction. The mixed gas intake can make the deposition more uniform without excessive deposition or under-deposition.
[0059] In order to further explain the technical solution of the present invention, the present invention is described in detail by specific embodiments below. In industrial production, considering the economic cost, argon is used as an inert gas for protection in the embodiments, and it can also be extended to other inert gases that do not participate in chemical reactions. The following examples will help researchers in the field to further understand the present invention, but do not limit the present invention in any form. It should be pointed out that for ordinary technicians in the field, some adjustments and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0060] The following test equipment uses general equipment unless otherwise specified, which does not affect the final result. The electron microscope is Thermo Fisher Apero2, the element analyzer is Thermo Fisher Flash 2000, and the ICP is Shimadzu ICPE-9000.
[0061] Example 1
[0062] The chemical vapor deposition equipment is a stainless steel reaction chamber.
[0063] The materials and reagents used are as follows: high-purity graphite blank (30mm*40mm*50mm), high-purity ethylene (99.999%), high-purity propylene (99.999%), high-purity hydrogen (99.999%), high-purity argon (99.999%); high-purity tantalum pentachloride (99.99%); the implementation steps are as follows:
[0064] (1) The chemical vapor deposition equipment is evacuated to a vacuum state of 500Pa and maintained at a vacuum state of 500Pa for 15 minutes. After checking that the chemical vapor deposition equipment is sealed intact, argon gas is introduced to fill the equipment to a normal pressure state, so that the argon gas fills the reaction chamber and all vacuum pipes. The gas valve is opened to evacuate the equipment, and argon gas is continued to be introduced for 10 minutes. The exhaust valve is closed. Through the above steps, various gases and impurities remaining in the chemical vapor deposition equipment are exhausted.
[0065] (2) After the high-purity graphite blank is cleaned with distilled water and dried at 170° C. for 8 hours, it is placed in the reaction chamber to ensure that the surface of the blank to be deposited faces the outlet direction of the reaction gas and that the blanks do not overlap or block each other;
[0066] (3) Evacuate to a vacuum state of 1000Pa and maintain the vacuum state of 1000Pa for 15 minutes. After checking that the vapor deposition equipment is sealed intact, introduce argon gas to fill it to normal pressure, so that the argon gas fills the reaction chamber and all vacuum pipes. Open the gas valve to evacuate, continue to introduce argon gas for 15 minutes, and close the exhaust valve. Through the above steps, various gases and impurities that enter the vapor deposition equipment during the placement of the blank are exhausted;
[0067] (4) Evacuate to a vacuum state of 1000Pa and maintain the vacuum state of 1000Pa for 10 minutes. After checking that the vapor deposition equipment is sealed intact, control the vacuum degree in the vapor deposition equipment to 3000Pa through a vacuum pump, and heat the temperature in the reaction chamber to 800°C;
[0068] (5) placing tantalum pentachloride in a vaporization chamber and heating it to 500° C. to vaporize it, and passing the vaporized tantalum pentachloride gas into a gas mixing tank. At the same time, passing hydrogen and argon into the gas mixing tank, the ratio of tantalum pentachloride, hydrogen and argon is 1:1:1, and the flow rates are 2SLM, 2SLM and 2SLM respectively. After being fully mixed in the gas mixing tank, passing them into a reaction chamber to carry out a chemical vapor deposition reaction on the blank for 5 hours; then cooling to 550° C., opening the mixed olefin valve, the mixed olefin flow rate is 2SLM, the vacuum is 5000Pa, and the reaction is carried out for 5 hours to prepare a tantalum-tantalum carbide coated graphite material;
[0069] (6) Disconnect the heating power supply and allow the reaction chamber to cool down naturally; when the temperature in the reaction chamber drops below 60°C, turn off the vacuum pump and continue to introduce argon. After the reaction chamber is filled to normal pressure, stop introducing argon, open the exhaust valve, open the reaction chamber, and take out the prepared tantalum carbide coated graphite material.
[0070] The thickness of the tantalum-tantalum carbide composite coating of the prepared tantalum carbide coated graphite material was tested using an electron microscope, and the test results showed that the coating thickness was 38μm. According to the ISO 4624-2016 coating adhesion test standard, the adhesion of the tantalum carbide coating of the prepared tantalum carbide coated graphite material was tested, and the peel strength was tested to be 25MPa, the graphite substrate was pulled apart, and the coating did not detach. Figure 1 This is a cross-sectional view of the composite coating of Example 1. Figure 4 This is the surface morphology of the tantalum carbide coating of Example 1. Figure 6 The metallographic images are dense and pore-free. The tantalum carbide coating was analyzed by X-ray photoelectron spectroscopy (XPS), and no other elements were found except Ta, C, and O. The oxygen element comes from the oxygen and carbon dioxide adsorbed by the sample in the atmosphere, which is difficult to remove in the XPS test.
[0071] Example 2
[0072] The chemical vapor deposition equipment is a stainless steel reaction chamber.
[0073] The materials and reagents used are as follows: high-purity graphite blank (30mm*40mm*50mm), high-purity ethylene (99.999%), high-purity propylene (99.999%), high-purity hydrogen (99.999%), high-purity argon (99.999%); high-purity tantalum pentachloride (99.99%); the implementation steps are as follows:
[0074] (1) The chemical vapor deposition equipment is evacuated to a vacuum state of 500Pa and maintained at a vacuum state of 500Pa for 15 minutes. After checking that the chemical vapor deposition equipment is sealed intact, argon gas is introduced to fill the equipment to a normal pressure state, so that the argon gas fills the reaction chamber and all vacuum pipes. The gas valve is opened to evacuate the equipment, and argon gas is continued to be introduced for 10 minutes. The exhaust valve is closed. Through the above steps, various gases and impurities remaining in the chemical vapor deposition equipment are exhausted.
[0075] (2) After the high-purity graphite blank is cleaned with distilled water and dried at 170° C. for 8 hours, it is placed in the reaction chamber to ensure that the surface of the blank to be deposited faces the outlet direction of the reaction gas and that the blanks do not overlap or block each other;
[0076] (3) Evacuate to a vacuum state of 1000Pa and maintain the vacuum state of 1000Pa for 15 minutes. After checking that the vapor deposition equipment is sealed intact, introduce argon gas to fill it to normal pressure, so that the argon gas fills the reaction chamber and all vacuum pipes. Open the gas valve to evacuate, continue to introduce argon gas for 15 minutes, and close the exhaust valve. Through the above steps, various gases and impurities that enter the vapor deposition equipment during the placement of the blank are exhausted;
[0077] (4) Evacuate to 1000Pa vacuum state and maintain 1000Pa vacuum state for 10 minutes. After checking that the vapor deposition equipment is sealed intact, control the vacuum degree in the vapor deposition equipment to 6000Pa through a vacuum pump, and heat the temperature in the reaction chamber to 1100°C;
[0078] (5) placing tantalum pentachloride in a vaporization chamber and heating it to 500° C. to vaporize it, and passing the vaporized tantalum pentachloride gas into a gas mixing tank. At the same time, passing hydrogen and argon into the gas mixing tank, the ratio of tantalum pentachloride, hydrogen and argon is 1:2:1, and the flow rates are 2SLM, 4SLM and 2SLM respectively. After being fully mixed in the gas mixing tank, passing them into a reaction chamber to carry out a chemical vapor deposition reaction on the blank for 5 hours; then cooling to 550° C., opening the mixed olefin valve, the mixed olefin flow rate is 2SLM, the vacuum is 10000Pa, and the reaction is carried out for 5 hours to prepare a tantalum-tantalum carbide coated graphite material;
[0079] (6) Disconnect the heating power supply and allow the reaction chamber to cool down naturally; when the temperature in the reaction chamber drops below 60°C, turn off the vacuum pump and continue to introduce argon. After the reaction chamber is filled to normal pressure, stop introducing argon, open the exhaust valve, open the reaction chamber, and take out the prepared tantalum carbide coated graphite material.
[0080] The thickness of the tantalum-tantalum carbide composite coating of the prepared tantalum carbide coated graphite material was detected using an electron microscope, and the detection results showed that the coating thickness was 63μm. Figure 2-Figure 3 This is a cross-sectional view of the composite coating of Example 2. Figure 5 The surface morphology of the tantalum carbide coating of Example 1 is dense and pore-free. The tantalum carbide coating was analyzed by X-ray photoelectron spectroscopy (XPS), and no other elements were found except Ta, C, and O. The oxygen element comes from the oxygen and carbon dioxide adsorbed by the sample in the atmosphere, which is difficult to remove in the XPS test.
[0081] Example 3
[0082] The chemical vapor deposition equipment is a stainless steel reaction chamber.
[0083] The materials and reagents used are as follows: high-purity graphite blank (30mm*40mm*50mm), high-purity ethylene (99.999%), high-purity propylene (99.999%), high-purity hydrogen (99.999%), high-purity argon (99.999%); high-purity tantalum pentachloride (99.99%); the implementation steps are as follows:
[0084] (1) The chemical vapor deposition equipment is evacuated to a vacuum state of 500Pa and maintained at a vacuum state of 500Pa for 15 minutes. After checking that the chemical vapor deposition equipment is sealed intact, argon gas is introduced to fill the equipment to a normal pressure state, so that the argon gas fills the reaction chamber and all vacuum pipes. The gas valve is opened to evacuate the equipment, and argon gas is continued to be introduced for 10 minutes. The exhaust valve is closed. Through the above steps, various gases and impurities remaining in the chemical vapor deposition equipment are exhausted.
[0085] (2) After the high-purity graphite blank is cleaned with distilled water and dried at 170° C. for 8 hours, it is placed in the reaction chamber to ensure that the surface of the blank to be deposited faces the outlet direction of the reaction gas and that the blanks do not overlap or block each other;
[0086] (3) Evacuate to a vacuum state of 1000Pa and maintain the vacuum state of 1000Pa for 15 minutes. After checking that the vapor deposition equipment is sealed intact, introduce argon gas to fill it to normal pressure, so that the argon gas fills the reaction chamber and all vacuum pipes. Open the gas valve to evacuate, continue to introduce argon gas for 15 minutes, and close the exhaust valve. Through the above steps, various gases and impurities that enter the vapor deposition equipment during the placement of the blank are exhausted;
[0087] (4) Evacuate to 1000Pa vacuum state and maintain 1000Pa vacuum state for 10 minutes. After checking that the vapor deposition equipment is sealed intact, control the vacuum degree in the vapor deposition equipment to 6000Pa through a vacuum pump, and heat the temperature in the reaction chamber to 1100°C;
[0088] (5) placing tantalum pentachloride in a vaporization chamber and heating it to 500° C. to vaporize it, and passing the vaporized tantalum pentachloride gas into a gas mixing tank. At the same time, passing hydrogen and argon into the gas mixing tank, the ratio of tantalum pentachloride, hydrogen and argon is 1:2.5:1, and the flow rates are 6SLM, 15SLM and 6SLM respectively. After being fully mixed in the gas mixing tank, passing into a reaction chamber to carry out a chemical vapor deposition reaction on the blank for 5 hours; then cooling to 550° C., opening the mixed olefin valve, the mixed olefin flow rate is 12SLM, the vacuum is 10000Pa, and the reaction is carried out for 5 hours to prepare a tantalum-tantalum carbide coated graphite material;
[0089] (6) Disconnect the heating power supply and allow the reaction chamber to cool down naturally; when the temperature in the reaction chamber drops below 60°C, turn off the vacuum pump and continue to introduce argon. After the reaction chamber is filled to normal pressure, stop introducing argon, open the exhaust valve, open the reaction chamber, and take out the prepared tantalum carbide coated graphite material.
[0090] The thickness of the tantalum-tantalum carbide composite coating of the prepared tantalum carbide coated graphite material was tested using an electron microscope, and the test results showed that the coating thickness was 118μm. According to the ISO 4624-2016 coating adhesion test standard, the adhesion of the tantalum carbide coating of the prepared tantalum-tantalum carbide composite coated graphite material was tested. The peel strength was tested to be 24MPa, the graphite substrate was pulled apart, and the coating did not detach. The tantalum carbide coating was analyzed by X-ray photoelectron spectroscopy (XPS), and it was determined that there were no other elements except Ta, C, and O. The oxygen element comes from the oxygen and carbon dioxide adsorbed by the sample in the atmosphere, which is difficult to remove in the XPS test. The surface morphology of the coating was observed by scanning electron microscopy, which was dense and without pores or cracks.
[0091] Example 4
[0092] The chemical vapor deposition equipment is a stainless steel reaction chamber.
[0093] The materials and reagents used are as follows: high-purity carbon / carbon blank (30mm*40mm*50mm), high-purity ethylene (99.999%), high-purity propylene (99.999%), high-purity hydrogen (99.999%), high-purity argon (99.999%); high-purity tantalum pentachloride (99.99%); the implementation steps are as follows:
[0094] (1) The chemical vapor deposition equipment is evacuated to a vacuum state of 500Pa and maintained at a vacuum state of 500Pa for 15 minutes. After checking that the chemical vapor deposition equipment is sealed intact, argon gas is introduced to fill the equipment to a normal pressure state, so that the argon gas fills the reaction chamber and all vacuum pipes. The gas valve is opened to evacuate the equipment, and argon gas is continued to be introduced for 10 minutes. The exhaust valve is closed. Through the above steps, various gases and impurities remaining in the chemical vapor deposition equipment are exhausted.
[0095] (2) After the high-purity carbon / carbon blank is cleaned with distilled water and dried at 170° C. for 8 hours, it is placed in the reaction chamber to ensure that the surface of the blank to be deposited faces the outlet direction of the reaction gas and that the blanks do not overlap or block each other;
[0096] (3) Evacuate to a vacuum state of 1000Pa and maintain the vacuum state of 1000Pa for 15 minutes. After checking that the vapor deposition equipment is sealed intact, introduce argon gas to fill it to normal pressure, so that the argon gas fills the reaction chamber and all vacuum pipes. Open the gas valve to evacuate, continue to introduce argon gas for 15 minutes, and close the exhaust valve. Through the above steps, various gases and impurities that enter the vapor deposition equipment during the placement of the blank are exhausted;
[0097] (4) Evacuate to a vacuum state of 1000Pa and maintain the vacuum state of 1000Pa for 10 minutes. After checking that the vapor deposition equipment is sealed intact, control the vacuum degree in the vapor deposition equipment to 3000Pa through a vacuum pump, and heat the temperature in the reaction chamber to 800°C;
[0098] (5) placing tantalum pentachloride in a vaporization chamber and heating it to 500° C. to vaporize it, and passing the vaporized tantalum pentachloride gas into a gas mixing tank. At the same time, passing hydrogen and argon into the gas mixing tank, the ratio of tantalum pentachloride, hydrogen and argon is 1:1:1, and the flow rates are 2SLM, 2SLM and 2SLM respectively. After being fully mixed in the gas mixing tank, passing them into a reaction chamber to carry out a chemical vapor deposition reaction on the blank for 5 hours; then cooling to 750° C., opening the mixed olefin valve, the mixed olefin flow rate is 2SLM, the vacuum is 5000Pa, and the reaction is carried out for 5 hours to prepare a tantalum-tantalum carbide composite coating carbon / carbon material;
[0099] (6) Disconnect the heating power supply and allow the reaction chamber to cool down naturally; when the temperature in the reaction chamber drops below 60° C., turn off the vacuum pump and continue to introduce argon gas. After the reaction chamber is filled to normal pressure, stop introducing argon gas, open the exhaust valve, open the reaction chamber, and take out the prepared tantalum-tantalum carbide composite coating carbon / carbon material.
[0100] The thickness of the tantalum-tantalum carbide composite coating of the prepared tantalum carbide coated carbon / carbon material was detected using an electron microscope, and the test results showed that the coating thickness was 37μm. According to the ISO 4624-2016 coating adhesion test standard, the adhesion of the tantalum carbide coating of the prepared tantalum carbide coated carbon / carbon material was tested. The peel strength was tested to be 125MPa, the upper surface of the carbon / carbon substrate was peeled off, and the coating did not detach. The tantalum carbide coating was analyzed by X-ray photoelectron spectroscopy (XPS), and it was determined that there were no other elements except Ta, C, and O. The oxygen element comes from the oxygen and carbon dioxide adsorbed by the sample in the atmosphere, which is difficult to remove in the XPS test. The surface morphology of the coating was observed by scanning electron microscopy, which was dense and without pores or cracks.
[0101] Example 5
[0102] The chemical vapor deposition equipment is a stainless steel reaction chamber.
[0103] The materials and reagents used are as follows: high-purity silicon carbide blank (30mm*40mm*50mm), high-purity ethylene (99.999%), high-purity propylene (99.999%), high-purity hydrogen (99.999%), high-purity argon (99.999%); high-purity tantalum pentachloride (99.99%); the implementation steps are as follows:
[0104] (1) The chemical vapor deposition equipment is evacuated to a vacuum state of 500Pa and maintained at a vacuum state of 500Pa for 15 minutes. After checking that the chemical vapor deposition equipment is sealed intact, argon gas is introduced to fill the equipment to a normal pressure state, so that the argon gas fills the reaction chamber and all vacuum pipes. The gas valve is opened to evacuate the equipment, and argon gas is continued to be introduced for 10 minutes. The exhaust valve is closed. Through the above steps, various gases and impurities remaining in the chemical vapor deposition equipment are exhausted.
[0105] (2) After the high-purity silicon carbide blank is cleaned with distilled water and dried at 170° C. for 8 hours, it is placed in the reaction chamber to ensure that the surface of the blank to be deposited faces the outlet direction of the reaction gas and that the blanks do not overlap or block each other;
[0106] (3) Evacuate to a vacuum state of 1000Pa and maintain the vacuum state of 1000Pa for 15 minutes. After checking that the vapor deposition equipment is sealed intact, introduce argon gas to fill it to normal pressure, so that the argon gas fills the reaction chamber and all vacuum pipes. Open the gas valve to evacuate, continue to introduce argon gas for 15 minutes, and close the exhaust valve. Through the above steps, various gases and impurities that enter the vapor deposition equipment during the placement of the blank are exhausted;
[0107] (4) Evacuate to a vacuum state of 1000Pa and maintain the vacuum state of 1000Pa for 10 minutes. After checking that the vapor deposition equipment is sealed intact, control the vacuum degree in the vapor deposition equipment to 3000Pa through a vacuum pump, and heat the temperature in the reaction chamber to 800°C;
[0108] (5) placing tantalum pentachloride in a vaporization chamber and heating it to 500° C. to vaporize it, and passing the vaporized tantalum pentachloride gas into a gas mixing tank. At the same time, passing hydrogen and argon into the gas mixing tank, the ratio of tantalum pentachloride, hydrogen and argon is 1:1:1, and the flow rates are 2SLM, 2SLM and 2SLM respectively. After being fully mixed in the gas mixing tank, passing into a reaction chamber to carry out a chemical vapor deposition reaction on the blank for 5 hours; then opening the temperature to 750° C., mixing olefin valve, the mixed olefin flow rate is 2SLM, vacuum is 10000Pa, reacting for 5 hours, and preparing a tantalum-tantalum carbide composite coated silicon carbide material;
[0109] (6) Disconnect the heating power supply and allow the reaction chamber to cool down naturally; when the temperature in the reaction chamber drops below 60° C., turn off the vacuum pump and continue to introduce argon gas. After the reaction chamber is filled to normal pressure, stop introducing argon gas, open the exhaust valve, open the reaction chamber, and take out the prepared tantalum-tantalum carbide composite coated silicon carbide material.
[0110] The thickness of the tantalum-tantalum carbide composite coating of the prepared tantalum-tantalum carbide composite coating silicon carbide material was tested using an electron microscope, and the test results showed that the coating thickness was 35μm. According to the ISO 4624-2016 coating adhesion test standard, the adhesion of the tantalum-tantalum carbide coating of the prepared tantalum-tantalum carbide composite coating silicon carbide material was tested. The peel strength was tested to be 117MPa, the silicon carbide substrate was pulled apart, and the coating did not detach. The surface morphology of the coating was observed by scanning electron microscopy, and it was found that it was dense without pores or cracks. The tantalum carbide coating was analyzed by X-ray photoelectron spectroscopy (XPS), and it was determined that there were no other elements except Ta, C, and O. The oxygen element comes from the oxygen and carbon dioxide adsorbed by the sample in the atmosphere, which is difficult to remove in the XPS test.
[0111] Example 6
[0112] The chemical vapor deposition equipment is a stainless steel reaction chamber.
[0113] The materials and reagents used are as follows: high-purity graphite blank (30mm*40mm*50mm), high-purity ethylene (99.999%), high-purity propylene (99.999%), high-purity hydrogen (99.999%), high-purity argon (99.999%); high-purity tantalum pentafluoride (99.99%); the implementation steps are as follows:
[0114] (1) The chemical vapor deposition equipment is evacuated to a vacuum state of 500Pa and maintained at a vacuum state of 500Pa for 15 minutes. After checking that the chemical vapor deposition equipment is sealed intact, argon gas is introduced to fill the equipment to a normal pressure state, so that the argon gas fills the reaction chamber and all vacuum pipes. The gas valve is opened to evacuate the equipment, and argon gas is continued to be introduced for 10 minutes. The exhaust valve is closed. Through the above steps, various gases and impurities remaining in the chemical vapor deposition equipment are exhausted.
[0115] (2) After the high-purity graphite blank is cleaned with distilled water and dried at 170° C. for 8 hours, it is placed in the reaction chamber to ensure that the surface of the blank to be deposited faces the outlet direction of the reaction gas and that the blanks do not overlap or block each other;
[0116] (3) Evacuate to a vacuum state of 1000Pa and maintain the vacuum state of 1000Pa for 15 minutes. After checking that the vapor deposition equipment is sealed intact, introduce argon gas to fill it to normal pressure, so that the argon gas fills the reaction chamber and all vacuum pipes. Open the gas valve to evacuate, continue to introduce argon gas for 15 minutes, and close the exhaust valve. Through the above steps, various gases and impurities that enter the vapor deposition equipment during the placement of the blank are exhausted;
[0117] (4) Evacuate to a vacuum state of 1000Pa and maintain the vacuum state of 1000Pa for 10 minutes. After checking that the vapor deposition equipment is sealed intact, control the vacuum degree in the vapor deposition equipment to 3000Pa through a vacuum pump, and heat the temperature in the reaction chamber to 1100°C.
[0118] (5) placing tantalum pentafluoride in a vaporization chamber and heating it to 500° C. to vaporize it, and passing the vaporized tantalum pentachloride gas into a gas mixing tank. At the same time, passing hydrogen and argon into the gas mixing tank, the ratio of tantalum pentachloride, hydrogen and argon is 1:1:1, and the flow rates are 2SLM, 2SLM and 2SLM respectively. After being fully mixed in the gas mixing tank, passing them into a reaction chamber to carry out a chemical vapor deposition reaction on the blank for 5 hours; then cooling to 750° C., opening the mixed olefin valve, the mixed olefin flow rate is 2SLM, the vacuum is 10000Pa, and the reaction is carried out for 5 hours to prepare a tantalum-tantalum carbide coated graphite material;
[0119] (6) Disconnect the heating power supply and allow the reaction chamber to cool down naturally; when the temperature in the reaction chamber drops below 60°C, turn off the vacuum pump and continue to introduce argon. After the reaction chamber is filled to normal pressure, stop introducing argon, open the exhaust valve, open the reaction chamber, and take out the prepared tantalum carbide coated graphite material.
[0120] The thickness of the tantalum-tantalum carbide composite coating of the prepared tantalum carbide coated graphite material was tested using an electron microscope, and the test results showed that the coating thickness was 38μm. According to the ISO 4624-2016 coating adhesion test standard, the adhesion of the tantalum carbide coating of the prepared tantalum carbide coated graphite material was tested. The peel strength was 27MPa, the graphite substrate was pulled apart, and the coating did not detach. The surface morphology of the coating was observed by scanning electron microscopy, which was dense without pores or cracks. The tantalum carbide coating was analyzed by X-ray photoelectron spectroscopy (XPS), and it was determined that there were no other elements except Ta, C, and O. The oxygen element comes from the oxygen and carbon dioxide adsorbed by the sample in the atmosphere, which is difficult to remove in the XPS test.
[0121] The above embodiments and drawings do not limit the product form and style of the present invention. Any appropriate changes or modifications made by ordinary technicians in the relevant technical field, such as changes in parameters such as reaction temperature, vaporization temperature, gas flow rate, etc., should be deemed to be within the patent scope of the present invention.
Claims
1. A method for preparing a tantalum-tantalum carbide composite coating, forming a tantalum-tantalum carbide composite coating on a substrate by chemical vapor deposition, It is characterized in that The following steps are involved: ① Heating step: placing the substrate in a CVD reaction chamber, evacuating the reaction chamber, and heating the reaction chamber, wherein the heating temperature is 800 to 1100° C.; ② Tantalum coating deposition step: after the heating step, tantalum pentachloride or tantalum pentafluoride is gasified and introduced into a reaction chamber with hydrogen, maintained at a pressure of 3000Pa to 6000Pa and a reaction temperature of 800 to 1100°C, to deposit a tantalum coating on the surface of the substrate; ③ Cooling step: stop introducing the reaction gas, cool down, and start keeping warm when the temperature drops to 550-750℃; ④ Tantalum carbide coating deposition step: introducing tantalum pentachloride or tantalum pentafluoride gas, mixed olefin and hydrogen mixed gas into a reaction chamber, depositing tantalum carbide coating on the surface of tantalum coating at a pressure of 5000Pa to 10000Pa and a reaction temperature of 550 to 750°C to obtain tantalum-tantalum carbide composite coating material; the mixed olefin is a mixture of ethylene and propylene; the volume ratio of tantalum pentachloride or tantalum pentafluoride gas to hydrogen is 1:1 to 2.5; the volume ratio of tantalum pentachloride or tantalum pentafluoride gas to mixed olefin is 1:1 to 2; the volume ratio of ethylene to propylene in the mixed olefin is 1:1 to 2; ⑤Cooling step: After the above steps, the tantalum-tantalum carbide coated product is cooled to room temperature.
2. The method for preparing a tantalum-tantalum carbide composite coating according to claim 1, Features: The gasification temperature of the tantalum pentachloride or tantalum pentafluoride is 300-600°C.
3. The method for preparing a tantalum-tantalum carbide composite coating according to claim 1, Features: The volume ratio of tantalum pentachloride or tantalum pentafluoride gas to hydrogen in step ② is 1:1 to 2.
5.
4. The method for preparing a tantalum-tantalum carbide composite coating according to claim 1, Features: The flow rate of the tantalum pentachloride or tantalum pentafluoride gas is 2-6 SLM, the flow rate of the mixed olefin gas is 2-12 SLM, and the flow rate of the hydrogen gas is 2-15 SLM.
5. The method for preparing a tantalum-tantalum carbide composite coating according to claim 1, Features: In step ②, the tantalum pentachloride or tantalum pentafluoride gas is introduced into the reaction chamber through a carrier gas, and the carrier gas is argon; the volume ratio of the tantalum pentachloride or tantalum pentafluoride gas to the carrier gas is 1:1-3.
6. The method for preparing a tantalum-tantalum carbide composite coating according to claim 1, Features: The reaction chamber is a stainless steel reaction chamber.
7. The method for preparing a tantalum-tantalum carbide composite coating according to claim 1, Features: The substrate is a metal material, a carbon material, a ceramic material or quartz.