A silicon wafer substrate surface pretreatment method and its application

By graphicizing, magnetron sputtering molybdenum plating and ultrasonic oscillation treatment on the surface of the silicon wafer, regular nucleation areas and scratch defects are formed, which solves the structural unevenness and stress of the diamond film, and improves the yield rate of the film and Stability of the substrate.

CN115637431BActive Publication Date: 2024-11-19WUHAN LEGER CRYSTAL DIAMOND TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211334890.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-28
Publication Date
2024-11-19
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

In the deposition and preparation of diamond films, the unsatisfactory surface pretreatment of the silicon wafer leads to uneven structure of the diamond film, causing stress and cracks, affecting the performance of the film and the stability of the substrate.

Method used

Use graphical processing, magnetron sputtering molybdenum plating, glue removal and ultrasonic oscillation treatment to form regular mesh nucleation areas and uniform scratch defects, improve the nucleation density and uniformity of diamond films, and reduce the internal stress.

Benefits of technology

The nucleation rate and uniformity of the diamond film are significantly improved, and the chance of cracking of the substrate is reduced from 50% to below 10%, increasing the yield rate of the diamond film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003914355920000011
    Figure HDA0003914355920000011
  • Figure HDA0003914355920000021
    Figure HDA0003914355920000021
Patent Text Reader

Abstract

The present invention relates to a surface pretreatment method for a silicon wafer substrate, wherein a silicon wafer is used as a substrate, and patterning is performed on the surface thereof; the substrate obtained above is subjected to magnetron sputtering molybdenum plating treatment; the substrate obtained above is subjected to photoresist stripping treatment; the substrate obtained above is immersed in a diamond powder suspension for ultrasonic oscillation treatment to form scratch defects on the substrate surface; the substrate obtained above is cleaned and dried to obtain a target object. A silicon wafer substrate prepared by the surface pretreatment method for a silicon wafer substrate as described above is used to produce a self-supporting diamond film. The beneficial effect is: by patterning the surface of the silicon substrate to form a regularly arranged grid nucleation area, then a molybdenum transition layer is regularly deposited on the surface of the silicon substrate, and a diamond powder suspension is used to form uniform scratch defects on the patterned silicon wafer surface, thereby increasing the density and uniformity of diamond nucleation on the silicon wafer surface, and providing good prerequisites for the growth of high-quality diamond thick films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of heteroepitaxial diamond film materials, and in particular to a silicon wafer substrate surface pretreatment method and application thereof. Background Art

[0002] Diamond film has excellent comprehensive properties such as good wave transmittance from far infrared to ultraviolet, extremely high hardness and thermal conductivity, and excellent heat shock resistance, making it the most ideal infrared and X-ray window wave-transmitting material. Therefore, it has broad application prospects and is one of the most ideal materials for optical applications. The main goal of the military application of CVD diamond thick film is to develop a new generation of hypersonic interceptor missile hoods and infrared early warning, observation and aiming, and to improve the performance of infrared optical windows of various infrared weapon imaging devices so that they can adapt to working conditions in harsh battlefield environments and improve the battlefield survivability of the entire infrared weapon.

[0003] There is still a big gap between my country's research on the growth of thick diamond films and that of foreign countries. For the preparation of CVD thick diamond films, a more suitable growth substrate is usually required. Since the thermal expansion coefficient of the diamond film is small, when the thermal expansion coefficient of the substrate material is larger than that of the diamond, a large thermal stress will be generated between the substrate and the diamond, causing cracks in the film and thus affecting the performance of the film. Therefore, single crystal silicon wafers are usually used as substrates.

[0004] At present, in the deposition and preparation of diamond films, it is necessary to grind the surface of silicon wafers with diamond powder for a long time to improve the nucleation rate of diamond films during heteroepitaxial growth. The distribution, depth, length, etc. of grinding scratches on the surface of silicon wafers affect the growth orientation, surface morphology, structural uniformity, stress and other characteristics of diamond films to a certain extent.

[0005] It is very difficult to obtain evenly distributed grinding scratches on the surface of silicon wafers. When the pretreatment results of the silicon wafer surface are not ideal, as the thickness of the diamond film increases, the diamond film is prone to form uneven structural features, thereby generating greater stress and cracks. The substrate is also prone to warping and breaking, resulting in damage to the diamond film. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a silicon wafer substrate surface pretreatment method and application thereof, so as to overcome the deficiencies in the above-mentioned prior art.

[0007] The technical solution of the present invention to solve the above technical problem is as follows: A method for pretreating the surface of a silicon wafer substrate comprises the following steps:

[0008] S100, using a silicon wafer as a substrate, patterning the surface thereof to form a regularly arranged grid nucleation region;

[0009] S200, performing magnetron sputtering molybdenum plating treatment on the substrate obtained in S100;

[0010] S300, performing photoresist stripping treatment on the substrate obtained in S200;

[0011] S400, immersing the substrate obtained in S300 in a diamond powder suspension for ultrasonic vibration treatment to form scratch defects on the surface of the substrate;

[0012] S500, cleaning and drying the substrate obtained in S400 to obtain a target object.

[0013] Based on the above technical solution, the present invention can also be improved as follows.

[0014] Furthermore, the silicon wafer used in step S100 is first cleaned and dried, and then patterned.

[0015] Furthermore, the cleaning method is ultrasonic cleaning, and the parameters of the ultrasonic cleaning are set as follows: ultrasonic cleaning is performed using anhydrous ethanol, acetone and deionized water in sequence for 5 minutes to 10 minutes, and then drying is performed under a nitrogen atmosphere.

[0016] Furthermore, the mask used for patterning in step S100 includes patterns with a certain arrangement rule and regular shapes, and the distance between every two adjacent patterns is maintained at more than 30 μm.

[0017] Further, in step S200, the magnetron sputtering process is as follows: the sputtering gas is Ar, the flow rate thereof is controlled to be 15.0 mL / min, the sputtering gas pressure is maintained at 0.2 Pa to 0.4 Pa, the coating time is 15 min to 20 min, and the thickness of the plated molybdenum layer is controlled to be 0.3±0.1 μm.

[0018] Furthermore, the volume fraction of Ar is 99.999%.

[0019] Furthermore, the de-resisting process in step S300 is to immerse the substrate in an organic solvent to dissolve the photoresist.

[0020] Furthermore, the organic solvent is acetone, ethanol or amylethanol.

[0021] Furthermore, the average particle size of the diamond powder in the diamond powder suspension is 5±3 μm, and the solvent in the diamond powder suspension is ethanol, acetone or pentylethanol.

[0022] Furthermore, in step S500, the cleaning method is ultrasonic cleaning, and the parameters of the ultrasonic cleaning are set as follows: ultrasonic cleaning is performed using anhydrous ethanol, acetone and deionized water in sequence, and then drying is performed under a nitrogen atmosphere at a temperature controlled at 40° C. to 60° C.

[0023] The beneficial effects of the present invention are:

[0024] 1) The surface of the silicon substrate is patterned to form a regularly arranged grid nucleation area, and then a molybdenum transition layer is regularly deposited on the surface of the silicon substrate, and a diamond powder suspension is used to form uniform scratch defects on the patterned silicon wafer surface, thereby improving the density and uniformity of diamond nucleation on the silicon wafer surface, providing good prerequisites for the growth of high-quality diamond thick films;

[0025] 2) The transition layer of molybdenum is deposited regularly and evenly on the silicon substrate to increase the nucleation rate of the diamond film uniform nucleation, which can be generally 10 6 -10 7 The nucleation rate was increased to 10 9 -10 10 , which can effectively avoid the internal stress caused by the non-uniformity of nucleation rate;

[0026] 3) The process is simple, and the technologies used are relatively mature industrial production processes, which are suitable for mass industrial production and promotion.

[0027] Based on the above technical solution, the present invention also provides a target object prepared by the above silicon wafer substrate surface pretreatment method for use in producing a self-supporting diamond film.

[0028] The above further beneficial effects are: the obtained silicon wafer substrate has a lower thermal expansion coefficient, which reduces the probability of diamond film breakage. The present invention can reduce the probability of silicon wafer substrate breakage from 50% to less than 10%, solving the problem of the current technology that the prepared diamond film is prone to cracks and breakage due to unsatisfactory pretreatment process, thereby increasing the yield of diamond film growth.

[0029] Furthermore, the production method of the self-supporting diamond film is as follows: a silicon wafer substrate is placed in a microwave plasma chemical vapor deposition system, and after the gas pressure is pumped to 0.1 Pa, 300 sccm of hydrogen is introduced. When the pressure rises to 1 kPa, the microwave is turned on, the power and pressure are adjusted to make the temperature reading 850°C and the pressure 13 kPa, 6 sccm of methane is introduced, and after deposition for 120 hours, the obtained diamond film is immersed in a mixed solution of concentrated nitric acid and hydrofluoric acid to completely dissolve the silicon wafer substrate to obtain a self-supporting diamond film. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a flow chart of the silicon wafer substrate surface pretreatment method of the present invention;

[0031] Figure 2 This is a flow chart of the silicon wafer substrate surface pretreatment process described in the present invention. DETAILED DESCRIPTION

[0032] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0033] Example 1

[0034] like Figure 1 , Figure 2 As shown, a method for pretreating the surface of a silicon wafer substrate comprises the following steps:

[0035] S100, selecting a single crystal silicon wafer with a diameter of 50 mm as a substrate, using acetone, anhydrous ethanol, and deionized water to ultrasonically clean the substrate in sequence, then drying the single crystal silicon wafer with a diameter of 50 mm after ultrasonic cleaning in a nitrogen atmosphere, and then using a mask to pattern the surface of the obtained substrate to form a uniformly distributed pattern on the silicon deposited photoresist, and the mask used includes a regular square pattern arranged in longitude and latitude, each regular square pattern has a side length of 50 μm, and the spacing between every two adjacent square patterns is 50 μm;

[0036] S200, placing the substrate obtained in step S100 into a DC magnetron sputtering system, wherein the target material is metal molybdenum, the distance between the target material and the substrate is 80 mm, the sputtering gas is Ar (volume fraction is 99.999%), the flow rate is controlled to be 15.0 mL / min, the sputtering pressure is maintained at 0.3 Pa, and when the background vacuum of the vacuum chamber reaches 50 mPa, the sputtering coating is started, the time is 20 min, and the thickness of the plated molybdenum layer is 0.2 μm;

[0037] S300, soaking the substrate obtained in step S200 in acetone to completely remove the photoresist;

[0038] S400, placing the substrate obtained in step S300 into a diamond powder suspension, and ultrasonically treating it for 60 minutes to form scratch defects on the surface of the substrate, wherein the diamond powder suspension is prepared as follows: weighing 5g of diamond micropowder with an average particle size of 5±1.0μm and putting it into a beaker, and gradually dripping 100ml of anhydrous ethanol into the beaker to prepare a diamond powder suspension;

[0039] S500, the substrate obtained in step S400 is ultrasonically cleaned using acetone, anhydrous ethanol and deionized water in sequence for 15 minutes, and then placed in an oven and nitrogen is introduced, the temperature is set to 60°C, and dried.

[0040] The silicon wafer substrate after the above pretreatment is placed in a microwave plasma chemical vapor deposition system, and the mechanical vacuum pump is turned on to evacuate the gas pressure to 0.1 Pa, and then 300 sccm of hydrogen is introduced. When the pressure rises to 1 kPa, the microwave is turned on, and the power and pressure are adjusted to make the temperature reading 850°C and the pressure 13 kPa. 6 sccm of methane is introduced. After deposition for 120 hours, the obtained diamond film is immersed in a mixed solution of concentrated nitric acid and hydrofluoric acid to completely dissolve the silicon wafer substrate to obtain a self-supporting diamond film.

[0041] Example 2

[0042] like Figure 1 , Figure 2 As shown, a method for pretreating the surface of a silicon wafer substrate comprises the following steps:

[0043] S100, selecting a single crystal silicon wafer with a diameter of 100 mm as a substrate, using acetone, anhydrous ethanol, and deionized water to ultrasonically clean the substrate in sequence, then drying the single crystal silicon wafer with a diameter of 100 mm after ultrasonic cleaning in a nitrogen atmosphere, and then using a mask to pattern the surface of the obtained substrate to form a uniformly distributed pattern on the silicon deposited photoresist, and the mask used contains a regular rectangular pattern arranged in longitude and latitude, each regular rectangular pattern has a long side length of 50 μm, a short side length of 25 μm, and a spacing of 40 μm between every two adjacent rectangular patterns;

[0044] S200, placing the substrate obtained in step S100 into a DC magnetron sputtering system, wherein the target material is metal molybdenum, the distance between the target material and the substrate is 90 mm, the sputtering gas is Ar (volume fraction is 99.999%), the flow rate is controlled to be 15.0 mL / min, the sputtering pressure is maintained at 0.2 Pa, and when the background vacuum of the vacuum chamber reaches 40 mPa, the sputtering coating is started, the time is 15 min, and the thickness of the plated molybdenum layer is 0.2 μm;

[0045] S300, soaking the substrate obtained in step S200 in pentyl alcohol to completely remove the photoresist;

[0046] S400, placing the substrate obtained in step S300 into a diamond powder suspension, and ultrasonically treating it for 50 minutes to form scratch defects on the surface of the substrate, wherein the diamond powder suspension is prepared as follows: weighing 5g of diamond micropowder with an average particle size of 5±1.0μm and putting it into a beaker, and gradually dripping 100ml of pentylethanol into the beaker to prepare a diamond powder suspension;

[0047] S500, the substrate obtained in step S400 is ultrasonically cleaned using acetone, anhydrous ethanol and deionized water in sequence for 15 minutes, and then placed in an oven and nitrogen is introduced, the temperature is set to 60°C, and dried.

[0048] The silicon wafer substrate after the above pretreatment is placed in a microwave plasma chemical vapor deposition system, and the mechanical vacuum pump is turned on to evacuate the gas pressure to 0.1 Pa, and then 300 sccm of hydrogen is introduced. When the pressure rises to 1 kPa, the microwave is turned on, and the power and pressure are adjusted to make the temperature reading 850°C and the pressure 13 kPa. 6 sccm of methane is introduced. After deposition for 120 hours, the obtained diamond film is immersed in a mixed solution of concentrated nitric acid and hydrofluoric acid to completely dissolve the silicon wafer substrate to obtain a self-supporting diamond film.

[0049] Example 3

[0050] like Figure 1 , Figure 2 As shown, a method for pretreating the surface of a silicon wafer substrate comprises the following steps:

[0051] S100, selecting a single crystal silicon wafer with a diameter of 150 mm as a substrate, using acetone, anhydrous ethanol, and deionized water to ultrasonically clean the substrate in sequence, then drying the single crystal silicon wafer with a diameter of 150 mm after ultrasonic cleaning in a nitrogen atmosphere, and then using a mask to pattern the surface of the obtained substrate to form a uniformly distributed pattern on the silicon deposited photoresist, and the mask used includes a regular circular pattern arranged in longitude and latitude, each regular circular pattern has a diameter of 50 μm, and the spacing between every two adjacent circular patterns is 50 μm;

[0052] S200, placing the substrate obtained in step S100 into a DC magnetron sputtering system, wherein the target material is metal molybdenum, the distance between the target material and the substrate is 100 mm, the sputtering gas is Ar (volume fraction is 99.999%), the flow rate thereof is controlled to be 15.0 mL / min, the sputtering gas pressure is maintained at 0.4 Pa, and when the background vacuum of the vacuum chamber reaches 50 mPa, the sputtering coating is started, the time is 20 min, and the thickness of the plated molybdenum layer is 0.3 μm;

[0053] S300, soaking the substrate obtained in step S200 in acetone to completely remove the photoresist;

[0054] S400, placing the substrate obtained in step S300 into a diamond powder suspension, and ultrasonically treating it for 60 minutes to form scratch defects on the surface of the substrate, wherein the diamond powder suspension is prepared as follows: weighing 5g of diamond micropowder with an average particle size of 5±1.0μm and placing it into a beaker, and gradually dripping 100ml of acetone into the beaker to prepare a diamond powder suspension;

[0055] S500, the substrate obtained in step S400 is ultrasonically cleaned using acetone, anhydrous ethanol and deionized water in sequence for 15 minutes, and then placed in an oven and nitrogen is introduced, the temperature is set to 60°C, and dried.

[0056] The silicon wafer substrate after the above pretreatment is placed in a microwave plasma chemical vapor deposition system, and the mechanical vacuum pump is turned on to evacuate the gas pressure to 0.1 Pa, and then 300 sccm of hydrogen is introduced. When the pressure rises to 1 kPa, the microwave is turned on, and the power and pressure are adjusted to make the temperature reading 850°C and the pressure 13 kPa. 6 sccm of methane is introduced. After deposition for 120 hours, the obtained diamond film is immersed in a mixed solution of concentrated nitric acid and hydrofluoric acid to completely dissolve the silicon wafer substrate to obtain a self-supporting diamond film.

[0057] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for pretreating the surface of a silicon wafer substrate, characterized in that: The steps include: S100, using a silicon wafer as a substrate, patterning the surface of the obtained substrate using a mask, forming a uniformly distributed pattern on the photoresist deposited on the silicon to form a regularly arranged grid nucleation area, the mask used for patterning contains a pattern with a regular shape and arranged in longitude and latitude, and the spacing between every two adjacent patterns is maintained at more than 30 μm; S200, performing magnetron sputtering molybdenum plating treatment on the substrate obtained in S100, so that the molybdenum transition layer is regularly deposited on the surface of the silicon substrate to improve the nucleation rate of uniform nucleation of the diamond film and avoid internal stress caused by the non-uniformity of the nucleation rate; S300, performing photoresist stripping treatment on the substrate obtained in S200; S400, immersing the substrate obtained in S300 in a diamond powder suspension for ultrasonic oscillation treatment to form scratch defects on the surface of the substrate, so as to improve the density and uniformity of diamond nuclei on the surface of the silicon wafer; S500, cleaning and drying the substrate obtained in S400 to obtain the target object. The obtained silicon wafer substrate has a lower thermal expansion coefficient and reduces the probability of diamond film breakage when it is used to produce a self-supporting diamond film.

2. A method for pretreating a silicon wafer substrate surface according to claim 1, characterized in that: The silicon wafer used in step S100 is first cleaned and dried, and then patterned, wherein the cleaning method is ultrasonic cleaning, and the parameters of the ultrasonic cleaning are set as follows: ultrasonic cleaning is performed using anhydrous ethanol, acetone and deionized water in sequence for 5 minutes to 10 minutes, and then drying is performed in a nitrogen atmosphere.

3. The method for pretreating the surface of a silicon wafer substrate according to claim 1, characterized in that: The magnetron sputtering process in step S200 is as follows: the sputtering gas is Ar, the flow rate thereof is controlled to be 15.0 mL / min, the sputtering gas pressure is maintained at 0.2 Pa to 0.4 Pa, the coating time is 15 min to 20 min, and the thickness of the plated molybdenum layer is controlled to be 0.3±0.1 μm.

4. The method for pretreating the surface of a silicon wafer substrate according to claim 1, characterized in that: The de-resisting process in step S300 is to immerse the substrate in an organic solvent to dissolve the photoresist.

5. A silicon wafer substrate surface pretreatment method according to claim 4, characterized in that: The organic solvent is acetone, ethanol or pentylethanol.

6. The method for pretreating the surface of a silicon wafer substrate according to claim 1, characterized in that: The average particle size of the diamond powder in the diamond powder suspension is 5±3 μm, and the solvent in the diamond powder suspension is ethanol, acetone or pentylethanol.

7. The method for pretreating the surface of a silicon wafer substrate according to claim 1, characterized in that: The cleaning method in step S500 is ultrasonic cleaning, and the parameters of ultrasonic cleaning are set as follows: ultrasonic cleaning is performed using anhydrous ethanol, acetone and deionized water in sequence, and then drying is performed under a nitrogen atmosphere at a temperature controlled at 40° C. to 60° C.

8. A silicon wafer substrate prepared by the silicon wafer substrate surface pretreatment method according to any one of claims 1 to 7, used for producing a self-supporting diamond film.

9. The use according to claim 8, characterized in that: The production method of the self-supporting diamond film is as follows: The silicon wafer substrate was placed in a microwave plasma chemical vapor deposition system. After the gas pressure was pumped to 0.1Pa, 300sccm of hydrogen was introduced. When the pressure rose to 1KPa, the microwave was turned on, and the power and pressure were adjusted to make the temperature reading 850°C and the pressure 13KPa. 6sccm of methane was introduced. After deposition for 120 hours, the obtained diamond film was immersed in a mixed solution of concentrated nitric acid and hydrofluoric acid to completely dissolve the silicon wafer substrate to obtain a self-supporting diamond film.