Preparation process of fire-resistant and high-toughness special paper fiber felt
By soaking wet normal one-time pulp and glass fiber to make special thin felt, the existing fire-proof boards have solved the problem of cumbersome and low efficiency, and the efficient production of high-performance fire-proof materials has been achieved, reducing costs and energy consumption, and improving fire-proof and Impact resistance.
Patent Information
- Application Number
- CN202211373921.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-04
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing fire-resistant plates have cumbersome processes, low efficiency, high cost, poor fire resistance and insufficient impact resistance, which cannot meet the demand for high-toughness materials.
Wet normals are used to soak the pulp and glass fiber in one go to the fireproof slurry to make special thin felts. Through lamination or composite processes, fire-resistant materials with high fire resistance and strong impact resistance are obtained, which simplifies the process flow and reduces equipment investment and energy consumption.
It has achieved efficient production of materials with superior fire resistance, reduced equipment investment and energy consumption, improved production efficiency, compact products, flat surfaces, and improved flexural strength and fire resistance grade.
Smart Images

Figure CN115637610B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building material decoration, and in particular to a preparation process of fire-resistant and high-toughness special paper fiber felt. Background Art
[0002] Commonly used fireproof boards are mostly made of kraft paper impregnated with phenolic resin for the second time, or glass fiber cloth impregnated with resin for laminated molding. The fireproof and water-resistant furniture floors are also formed by hot pressing one or two impregnated kraft papers. The process is complicated, inefficient, and costly, and the fireproof performance is poor and the impact resistance is not strong. Therefore, in order to solve the above problems, it is particularly important to design a preparation process for fire-resistant and high-toughness special paper fiber felt. Summary of the invention
[0003] In order to solve the above problems, the present invention has designed a preparation process of a fire-resistant and high-toughness special paper fiber felt, which uses a wet line to soak paper pulp and glass fiber in fire-resistant slurry at one time to make a special thin felt. The special paper fiber felt can be directly laminated or compounded with furniture and floors to obtain a fire-resistant material with high fire resistance and strong impact resistance. This can not only reduce equipment investment and reduce costs, but also improve production efficiency.
[0004] In order to solve the above technical problems, the present invention provides a preparation process of a fire-resistant and high-toughness special paper fiber felt, which is characterized by comprising the following steps:
[0005] S1: preparing special slurry: taking 10-20 parts of resin, 10-30 parts of flame retardant, 50-80 parts of deionized water and 1-5 parts of additives by weight into a pressurized mixing tank, and mixing to obtain special slurry;
[0006] S2: preparing wet felt: mixing glass fiber and paper pulp, and forming on a forming net to obtain a wet felt;
[0007] S3: soaking slurry: transferring the wet felt blank prepared in step S2 from the forming net to the sizing net of the sizing machine, and evenly soaking the wet felt blank with special slurry through the sizing machine to obtain a glass fiber felt blank;
[0008] S4: Drying and curing: The glass fiber felt blank after being impregnated with glue is sent to a drying furnace for drying, and the finished product is obtained after drying.
[0009] Further: the resin in step S1 is one of phenolic resin, melamine formaldehyde resin, unsaturated polyester resin or urea formaldehyde resin.
[0010] Furthermore: the flame retardant in step S1 is one of aluminum hydroxide flame retardant, magnesium hydroxide flame retardant, ammonium polyphosphate flame retardant or aluminum hypophosphite flame retardant.
[0011] Furthermore: the auxiliary agent in step S1 is a dispersant and a coupling agent; the dispersant is one of fatty acids, aliphatic amides or esters; the coupling agent is a silane coupling agent, specifically one of KH550, KH560, KH570, KH792, DL602, and DL171.
[0012] Furthermore: in the step S2, the mixing ratio of glass fiber to pulp is 1-2:1, wherein the glass fiber is chopped glass fiber, the pulp is coniferous wood pulp or hardwood wood pulp, and the chopped glass fiber includes two types of 12mm and 6mm chopped glass fibers, and the specific ratio is: 2:1.
[0013] Furthermore: the drying temperature of the drying furnace is 180-200°C, the glass fiber felt blank after impregnation is placed on a translation trolley and enters and exits the drying furnace with the translation trolley, the speed of the translation trolley is 15-25m / min, the distance between the front and rear translation trolleys is 2-5m, and the drying time of each translation trolley is 1-3min.
[0014] Furthermore: the pressurized mixing tank in step S1 includes a tank body, a tank cover, a pressure unloading valve and a stirring motor, the left and right sides of the tank body are respectively provided with a first side panel and a second side panel, the left and right outer walls of the tank body are respectively rotatably connected between the first side panel and the second side panel through a rotating shaft, one of the rotating shafts passes through the second side panel and is connected to the servo motor, the stirring motor is installed at the center of the bottom of the tank body, the output shaft end of the stirring motor extends into the tank body and is connected to the stirring mechanism, the pressure unloading valve is also arranged at the bottom of the tank body, the tank cover is detachably installed at the upper end of the tank body, the tops of the first side panel and the second side panel are respectively embedded with electric push rods, the electric push rods are connected to the tank cover through a connecting piece, the tank cover is provided with a feed port and a pressurized pipe, and the pressurized pipe is connected to the pressurized tank through a sealed pipe joint.
[0015] Furthermore: a shower nozzle is arranged in the tank cover, and the shower nozzle is connected to a shower pipe connector arranged at the center of the top of the tank cover.
[0016] Furthermore: the pressure unloading valve comprises an outer valve body, an inner valve body, a valve core and a valve core spring, one end of the outer valve body is detachably fixed to the bottom of the tank body, the inner valve body is arranged in the outer valve body, the outer wall of the inner valve body fits the inner wall of the outer valve body and a spring clamping mechanism is arranged between each other, a protrusion is arranged at the end of the inner valve body away from the tank body, the end of the inner valve body away from the tank body is connected to the inner wall of the other end of the outer valve body through a compression spring, a limiting block is also arranged on the inner wall of the outer valve body below the inner valve body, a notch matching the protrusion is also arranged on the other end of the outer valve body, the protrusion extends out of the outer valve body along the notch and is movably connected with the outer valve body, and a spring clamping mechanism matching the valve core is arranged at the end of the inner valve body close to the tank body The guide groove is matched with the valve core, the valve core is connected in the guide groove through the valve core spring, the side wall of the guide groove is provided with a leakage hole that penetrates the inner valve body, the end of the protrusion extending out of the outer valve body is provided with a discharge hole, the leakage hole is connected with the discharge hole through a guide channel provided in the inner valve body, one end of the leakage hole is sealed by the valve core, and the other end of the leakage hole is sealed by the inner wall of the outer valve body, and a pressure relief discharge hole matching the leakage hole is also provided on the side wall of the outer valve body, the aperture of the leakage hole is larger than twice the aperture of the guide channel, and a filter screen is also provided in the outer valve body directly above the inner valve body, the valve core is facing the filter screen, and the filter screen is fixed to the outer valve body through an annular mounting plate provided on the outside thereof.
[0017] Furthermore: the spring clamping mechanism includes a clamping head and a clamping spring, the clamping head is composed of a trapezoidal clamping block and a guide part connected together, a guide hole matching the guide part is provided on the inner wall of the outer valve body, and a clamping groove matching the trapezoidal clamping block is provided on the outer wall of the inner valve body, the guide part is movably connected in the guide hole through the clamping spring, and the trapezoidal clamping block extends out of the guide hole and is clamped into the clamping groove under the action of the clamping spring.
[0018] After adopting the above design, the present invention uses a wet line to soak paper pulp and glass fiber in fireproof slurry to make a special thin felt at one time, and directly laminates with the special paper fiber felt, or compounds with furniture and floor to obtain a fireproof material with high fireproof performance and strong impact resistance, which can not only reduce equipment investment and reduce costs, but also improve production efficiency; the product is more dense and has a smooth surface without changing the thickness, and has the following advantages compared with conventional processes:
[0019] 1. Shorten the process: change from purchasing kraft paper and then dipping it in phenolic resin twice to one-time wet molding;
[0020] 2. Reduced energy consumption: Changing from the original two-time impregnation to the current one-time molding, the energy consumption is reduced by nearly half;
[0021] 3. Reduce equipment: Make full use of the glass fiber wet production line and save the equipment for secondary impregnation;
[0022] 4. Better product performance: Glass fiber significantly improves the flexural strength of fireproof panels; mixed with glass fiber, it is more resistant to high temperatures than kraft paper; compared with phenolic impregnated kraft paper, this felt can achieve Class A fireproofing;
[0023] 5. Easy to use: It can be formed by directly laminating or pasting furniture or floors with special paper fiber felt at one time. It also has the properties of fire resistance, water resistance and impact resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0025] Figure 1 It is a schematic diagram of the structure of a pressurized mixing tank.
[0026] Figure 2 This is the structural diagram of the pressure unloading valve.
[0027] Figure 3 for Figure 2 A is an enlarged view of the middle image. DETAILED DESCRIPTION
[0028] The present invention provides a preparation process of a fire-resistant and high-toughness special paper fiber felt, which specifically comprises the following steps:
[0029] S1: preparing special slurry: taking 10-20 parts of resin, 10-30 parts of flame retardant, 50-80 parts of deionized water and 1-5 parts of additives by weight into a pressurized mixing tank, and mixing to obtain special slurry;
[0030] S2: preparing wet felt: mixing glass fiber and paper pulp, and forming on a forming net to obtain a wet felt;
[0031] S3: soaking slurry: transferring the wet felt blank prepared in step S2 from the forming net to the sizing net of the sizing machine, and evenly soaking the wet felt blank with special slurry through the sizing machine to obtain a glass fiber felt blank;
[0032] S4: Drying and curing: The glass fiber felt blank after being impregnated with glue is sent to a drying furnace for drying, and the finished product is obtained after drying.
[0033] The resin in the above step S1 is one of phenolic resin, melamine formaldehyde resin, unsaturated polyester resin or urea formaldehyde resin.
[0034] The flame retardant in the above step S1 is one of aluminum hydroxide flame retardant, magnesium hydroxide flame retardant, ammonium polyphosphate flame retardant or aluminum hypophosphite flame retardant.
[0035] The auxiliary agents in the above step S1 are dispersants and coupling agents; the dispersant is one of fatty acids, aliphatic amides or esters; the coupling agent is a silane coupling agent, specifically one of KH550, KH560, KH570, KH792, DL602, and DL171.
[0036] In the above step S2, the mixing ratio of glass fiber and pulp is 1-2:1, wherein the glass fiber is chopped glass fiber, and the pulp is coniferous wood pulp or hardwood pulp. The chopped glass fiber includes two types of 12mm and 6mm chopped glass fibers, and the specific ratio is: 2:1.
[0037] The drying temperature of the above-mentioned drying furnace is 180-200°C. The glass fiber felt blank after impregnation is placed on a translation trolley and enters and exits the drying furnace with the translation trolley. The speed of the translation trolley is 15-25m / min, the distance between the front and rear translation trolleys is 2-5m, and the drying time of each translation trolley is 1-3min.
[0038] In summary, the present invention utilizes a wet process to soak paper pulp and glass fiber in fireproof slurry to form a special thin felt at one time, and directly laminates the special paper fiber felt, or compounds it with furniture and flooring to obtain a fireproof material with high fireproof performance and strong impact resistance, which can not only reduce equipment investment and reduce costs, but also improve production efficiency; the product is more compact and has a smooth surface without changing the thickness, and has the following advantages compared with conventional processes: 1. The process is shortened: the original purchase of kraft paper and then secondary impregnation with phenolic resin is changed to one-time wet molding; 2. Reduced energy consumption: Energy consumption is reduced by nearly half by changing from the original two-time impregnation to the current one-time molding; 3. Reduced equipment: Fully utilize the glass fiber wet process production line to eliminate the equipment for the second impregnation; 4. Better product performance: Glass fiber significantly improves the flexural strength of fireproof panels; after mixing with glass fiber, it is more resistant to high temperatures than kraft paper; compared with phenolic impregnated kraft paper, this felt can achieve Class A fire protection; 5. Easy to use: Special paper fiber felt can be directly laminated or pasted on furniture or floors in one go to form, and it also has fireproof, water-resistant and impact-resistant properties.
[0039] like Figure 1The pressurized mixing tank in step S1 shown includes a tank body 3, a tank cover 4, a pressure unloading valve 13 and a stirring motor 12, wherein the left and right sides of the tank body are respectively provided with a first side panel 1 and a second side panel 2, and the left and right outer walls of the tank body are respectively rotatably connected between the first side panel and the second side panel through a rotating shaft, wherein one rotating shaft passes through the second side panel and is connected to the servo motor, and the stirring motor is installed at the center of the bottom of the tank body, and the output shaft end of the stirring motor extends into the tank body and is connected to the stirring mechanism, and the pressure unloading valve is also arranged at the bottom of the tank body, and the tank cover is detachably installed at the upper end of the tank body, and the tops of the first side panel and the second side panel are respectively embedded with electric push rods 6, and the electric push rods are connected to the tank cover through a connecting piece 7, and a feed port 5 and a pressurized pipe 9 are provided on the tank cover, and the pressurized pipe is connected to the pressurized tank through a sealed pipe joint 10.
[0040] like Figure 1 The tank cover shown is provided with a shower nozzle, which is connected to a shower pipe connector 11 provided at the center of the top of the tank cover.
[0041] like Figure 2The pressure unloading valve shown includes an outer valve body 13-1, an inner valve body 13-2, a valve core 13-5 and a valve core spring 13-6, one end of the outer valve body is detachably fixed to the bottom of the tank body, the inner valve body is arranged in the outer valve body, the outer wall of the inner valve body fits the inner wall of the outer valve body and a spring clamping mechanism is arranged between each other, a protrusion 13-11 is arranged at the end of the inner valve body away from the tank body, the end of the inner valve body away from the tank body is connected to the inner wall of the other end of the outer valve body through a compression spring 13-10, a limiting block 13-13 is also arranged on the inner wall of the outer valve body below the inner valve body, a notch matching the protrusion is also arranged on the other end of the outer valve body, the protrusion extends out of the outer valve body along the notch and is movably connected with the outer valve body, and a valve core matching the valve core is arranged at the end of the inner valve body close to the tank body A matching guide groove, the valve core is connected in the guide groove through a valve core spring, a leakage hole 13-7 penetrating the inner valve body is provided on the side wall of the guide groove, a discharge hole 13-12 is provided on one end of the protrusion extending out of the outer valve body, the leakage hole is connected with the discharge hole through a guide channel 13-9 provided in the inner valve body, one end of the leakage hole is sealed by the valve core, and the other end of the leakage hole is sealed by the inner wall of the outer valve body, a pressure relief discharge hole 13-8 matching the leakage hole is also provided on the side wall of the outer valve body, the aperture of the leakage hole is larger than twice the aperture of the guide channel, a filter screen 13-3 is also provided in the outer valve body directly above the inner valve body, the valve core is facing the filter screen, and the filter screen is fixed to the outer valve body through an annular mounting plate 13-4 provided on its outside. When the discharge hole is blocked or the pressure in the tank is too high, the spring clamping mechanism will automatically open under the action of excessive pressure, so that the discharge hole is directly opposite to the pressure relief discharge hole under the action of the limit block, thereby performing pressure relief and unloading through the pressure relief discharge hole, which increases practical performance.
[0042] like Figure 3 The spring clamping mechanism shown includes a clamping head and a clamping spring 13-16, wherein the clamping head is composed of a trapezoidal clamping block 13-14 and a guide portion 13-15 connected together as a whole, a guide hole matching the guide portion is provided on the inner wall of the outer valve body, and a clamping groove matching the trapezoidal clamping block is provided on the outer wall of the inner valve body, the guide portion is movably connected in the guide hole through the clamping spring, and the trapezoidal clamping block extends out of the guide hole and is clamped into the clamping groove under the action of the clamping spring.
[0043] Embodiment 1:
[0044] A1: Prepare special slurry: 20 parts of phenolic resin, 20 parts of aluminum hydroxide, 59 parts of deionized water, 0.5 parts of dispersant, 0.5 parts of coupling agent KH550, and stir at high speed at room temperature and pressure for half an hour;
[0045] A2: preparing wet felt: glass fiber and softwood pulp are mixed in a ratio of 1:1, and formed on a forming net to obtain a wet felt;
[0046] A3: Impregnation with slurry: The wet felt blank prepared in step A2 is transferred from the forming net to the sizing net of the sizing machine, and the special slurry prepared in step 1 is evenly impregnated on the wet felt blank by the sizing machine to obtain a glass fiber felt blank;
[0047] A4: Drying and curing. The glass fiber felt blank after impregnation is sent to the drying oven for drying. The speed is 20m / min and the oven temperature is 200℃. The finished product is rolled up. The finished special felt has a gram weight of 500g / ㎡, a thickness of 0.5mm, and a fire protection grade of A.
[0048] Embodiment 2:
[0049] B1: Prepare special slurry: 10 parts of melamine formaldehyde resin, 40 parts of magnesium hydroxide, 49 parts of deionized water, 0.5 parts of dispersant, 0.5 parts of coupling agent KH560, and stir at high speed at room temperature and pressure for half an hour;
[0050] B2: preparing wet felt: glass fiber and softwood pulp are mixed in a ratio of 2:1 and formed on a forming net to obtain a wet felt;
[0051] B3: Impregnation with slurry: The wet felt blank prepared in step B2 is transferred from the forming net to the sizing net of the sizing machine, and the special slurry prepared in step 1 is evenly impregnated on the wet felt blank by the sizing machine to obtain a glass fiber felt blank;
[0052] B4: Drying and curing. The glass fiber felt blank after impregnation is sent to the drying oven for drying at a speed of 15m / min and an oven temperature of 200℃. The finished product is rolled up. The finished special felt has a gram weight of 500g / ㎡, a thickness of 0.5mm, and a fire protection grade of A.
[0053] The above are only preferred embodiments of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should be regarded as the protection scope of the present invention.
Claims
1. A preparation process of fire-resistant and high-toughness special paper fiber felt, characterized in that: The specific steps include: S1: preparing special slurry: taking 10-20 parts of resin, 10-30 parts of flame retardant, 50-80 parts of deionized water and 1-5 parts of additives by weight into a pressurized mixing tank, and mixing to obtain special slurry; S2: preparing wet felt: mixing glass fiber and paper pulp, and forming on a forming net to obtain a wet felt; S3: soaking slurry: transferring the wet felt blank prepared in step S2 from the forming net to the sizing net of the sizing machine, and evenly soaking the wet felt blank with special slurry through the sizing machine to obtain a glass fiber felt blank; S4: Drying and curing: The glass fiber felt blank after impregnation is sent to a drying furnace for drying, and the finished product is obtained after drying; The resin in step S1 is one of phenolic resin, melamine formaldehyde resin, unsaturated polyester resin or urea formaldehyde resin; The flame retardant in step S1 is one of aluminum hydroxide flame retardant, magnesium hydroxide flame retardant, ammonium polyphosphate flame retardant or aluminum hypophosphite flame retardant; The auxiliary agents in step S1 are dispersants and coupling agents; the dispersant is one of fatty acids, aliphatic amides or esters; the coupling agent is a silane coupling agent, specifically one of KH550, KH560, KH570, KH792, DL602, and DL171; In step S2, the mixing ratio of glass fiber to pulp is 1-2:1, wherein the glass fiber is chopped glass fiber, and the pulp is coniferous wood pulp or hardwood wood pulp. The chopped glass fiber includes two types of 12 mm and 6 mm chopped glass fibers, and the specific ratio is 2:1; The drying temperature of the drying furnace is 180-200°C. The glass fiber felt after the dip is placed on a translation trolley and enters and exits the drying furnace with the translation trolley. The speed of the translation trolley is 15-25m / min. The distance between the front and rear translation trolleys is 2-5m. The drying time of each translation trolley is 1-3min. The pressurized mixing tank in step S1 comprises a tank body (3), a tank cover (4), a pressure discharge valve (13) and a stirring motor (12), wherein the left and right sides of the tank body are respectively provided with a first side plate (1) and a second side plate (2), and the left and right outer walls of the tank body are respectively rotatably connected between the first side plate and the second side plate through a rotating shaft, wherein one rotating shaft passes through the second side plate and is connected to the servo motor, and the stirring motor is installed at the center of the bottom of the tank body, and the shaft end of the stirring motor extends into the tank body and is connected to the stirring mechanism, and the pressure A force discharge valve is also arranged at the bottom of the tank body, the tank cover is detachably mounted on the upper end of the tank body, the tops of the first side plate and the second side plate are respectively embedded with electric push rods (6), the electric push rods are connected to the tank cover through a connector (7), the tank cover is provided with a feed port (5) and a pressurizing pipe (9), the pressurizing pipe is connected to the pressurizing tank through a sealing pipe joint (10); a shower nozzle is arranged inside the tank cover, the shower nozzle is connected to a shower pipe connector (11) arranged at the center of the top of the tank cover; The pressure unloading valve comprises an outer valve body (13-1), an inner valve body (13-2), a valve core (13-5) and a valve core spring (13-6); one end of the outer valve body is detachably fixed to the bottom of the tank body; the inner valve body is arranged in the outer valve body; the outer wall of the inner valve body fits the inner wall of the outer valve body and a spring clamping mechanism is arranged between them; a protrusion (13-11) is arranged at one end of the inner valve body away from the tank body; the end of the inner valve body away from the tank body is connected to the inner wall of the other end of the outer valve body through a compression spring (13-10); a limit block (13-13) is also arranged on the inner wall of the outer valve body below the inner valve body; a notch matching the protrusion is also arranged on the other end of the outer valve body; the protrusion extends out of the outer valve body along the notch and is movably connected to the outer valve body; and a valve core spring is provided at one end of the inner valve body close to the tank body. A guide groove is matched with the guide groove, the valve core is connected to the guide groove through a valve core spring, a leakage hole (13-7) penetrating the inner valve body is provided on the side wall of the guide groove, a discharge hole (13-12) is provided on one end of the protruding portion extending out of the outer valve body, the leakage hole is connected to the discharge hole through a guide channel (13-9) provided inside the inner valve body, one end of the leakage hole is sealed by the valve core, and the other end of the leakage hole is sealed by the inner wall of the outer valve body, a pressure relief discharge hole (13-8) matching the leakage hole is also provided on the side wall of the outer valve body, the aperture of the leakage hole is larger than one times the aperture of the guide channel, a filter screen (13-3) is also provided in the outer valve body directly above the inner valve body, the valve core is directly facing the filter screen, and the filter screen is fixed in the outer valve body through an annular mounting plate (13-4) provided outside the filter screen; The spring clamping mechanism comprises a clamping head and a clamping spring (13-16); the clamping head is composed of a trapezoidal clamping block (13-14) and a guide part (13-15) connected together; a guide hole matching the guide part is provided on the inner wall of the outer valve body; a clamping groove matching the trapezoidal clamping block is provided on the outer wall of the inner valve body; the guide part is movably connected in the guide hole through the clamping spring; and the trapezoidal clamping block extends out of the guide hole and is clamped in the clamping groove under the action of the clamping spring.
Citation Information
Patent Citations
A1-grade non-combustible composite and preparation method thereof
CN106316215A
Structural flame-retardant functional composite material and preparation method thereof
CN112009038A
Fireproof antibacterial special functional plate and preparation method thereof
CN112622369A
High-acid-leakage-height glass fiber felt and preparation method thereof
CN112695567A
Lightweight thermal-insulation high-toughness fireproof plate and preparation method thereof
CN113233918A