A water-soluble high-efficiency degreasing agent and preparation method thereof
By using water-soluble and efficient oil degreaser of specific formulas, the problems of water-soluble and low efficiency of oil degreaser in industrial circulation water systems are solved, and the effects of oil removal, descaling, sterilization and corrosion prevention are achieved, and phosphorus pollution is avoided. Simplifies the cleaning process.
Patent Information
- Application Number
- CN202211400394.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-11-09
AI Technical Summary
Existing oil degreasers have problems such as poor water solubility, low efficiency or phosphorus contaminants in industrial circulating water systems, resulting in complex and high cost.
A modified from sodium dodecylbenzene sulfonate, nonylphenol polyoxyethylene ether NP-10, fatty alcohol polyoxyethylene ether JFC, polyepoxysuccinic acid, disodium ethylenediaminetetraacetic acid, and polyether The water-soluble and efficient oil removal agent formula consisting of silicone defoaming agent, sodium hydroxide, isothiazolinone and TTA is prepared through a specific stirring and heating process to ensure the reasonable compatibility and operating conditions of each component.
The high-efficiency water-soluble, descaling, sterilization and corrosion-proof effects of oil degassing agents are achieved, while avoiding phosphorus pollution. The preparation method is simple, environmentally friendly, and no waste discharge.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal surface treatment agent preparation, and in particular to a water-soluble high-efficiency degreasing agent and a preparation method thereof. Background Art
[0002] After the equipment is installed or the system leaks oil, the industrial circulating water system often needs to be cleaned chemically to remove the oil on the surface of the equipment. At this time, a degreasing agent is often used. However, the degreasing agents on the market often have defects such as poor water solubility, low efficiency, or phosphorus pollutants, which makes the cleaning process complicated or increases the cleaning cost. Therefore, it is particularly necessary to develop a water-soluble and efficient degreasing agent.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] The first purpose of the present invention is to provide a water-soluble high-efficiency degreasing agent with a simple formula, which solves the above-mentioned problems, has good water solubility, high degreasing efficiency, and has the effects of sterilization, anti-scaling, anti-corrosion and simple preparation.
[0005] The second object of the present invention is to provide a method for preparing the above-mentioned water-soluble high-efficiency oil remover, which has simple operation, mild operating conditions, no pollution, no discharge of three wastes, and is safe and environmentally friendly.
[0006] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0007] The invention provides a water-soluble high-efficiency oil remover, which is mainly prepared from the following raw materials: by weight, 8-10 parts of sodium dodecylbenzene sulfonate, 12-18 parts of nonylphenol polyoxyethylene ether NP-10, 6-8 parts of fatty alcohol polyoxyethylene ether JFC, 10-14 parts of polyepoxysuccinic acid, 5-10 parts of disodium ethylenediaminetetraacetic acid, 1-3 parts of polyether modified silicone defoamer, 3-6 parts of sodium hydroxide, 2-4 parts of isothiazolinone, 0.1-0.3 parts of TTA and 10-20 parts of deionized water.
[0008] Preferably, as a further feasible scheme, in parts by mass, 9-10 parts of sodium dodecylbenzene sulfonate, 13-17 parts of nonylphenol polyoxyethylene ether NP-10, 7-8 parts of fatty alcohol polyoxyethylene ether JFC, 11-13 parts of polyepoxysuccinic acid, 6-9 parts of disodium ethylenediaminetetraacetic acid, 2-3 parts of polyether modified silicone defoamer, 4-5 parts of sodium hydroxide, 3-4 parts of isothiazolinone, 0.2-0.3 parts of TTA, and 11-19 parts of deionized water.
[0009] Preferably, as a further feasible scheme, in parts by mass, 9 parts of sodium dodecylbenzene sulfonate, 14 parts of nonylphenol polyoxyethylene ether NP-10, 7 parts of fatty alcohol polyoxyethylene ether JFC, 11 parts of polyepoxysuccinic acid, 6 parts of disodium ethylenediaminetetraacetic acid, 2 parts of polyether modified silicone defoamer, 4 parts of sodium hydroxide, 3 parts of isothiazolinone, 0.2 parts of TTA, and 11 parts of deionized water.
[0010] Preferably, as a further feasible scheme, in parts by mass, 10 parts of sodium dodecylbenzene sulfonate, 15 parts of nonylphenol polyoxyethylene ether NP-10, 8 parts of fatty alcohol polyoxyethylene ether JFC, 13 parts of polyepoxysuccinic acid, 9 parts of disodium ethylenediaminetetraacetic acid, 3 parts of polyether modified silicone defoamer, 5 parts of sodium hydroxide, 4 parts of isothiazolinone, 0.3 parts of TTA, and 19 parts of deionized water.
[0011] The above-mentioned water-soluble high-efficiency degreasing agent formula includes sodium dodecylbenzene sulfonate, nonylphenol polyoxyethylene ether NP-10, fatty alcohol polyoxyethylene ether JFC, polyepoxysuccinic acid, disodium ethylenediaminetetraacetic acid, polyether modified silicone defoamer, sodium hydroxide, isothiazolinone, TTA, and deionized water. The functions of each raw material are as follows:
[0012] 1. Sodium dodecylbenzene sulfonate: It has strong foaming power, high detergency, is easy to compound with various additives, has low cost, and is an excellent anionic surfactant.
[0013] 2. Nonylphenol polyoxyethylene ether NP-10: It is a non-ionic surfactant, mainly used as an emulsifier, detergent, wetting agent, dispersant and defoaming agent.
[0014] 3. Fatty alcohol polyoxyethylene ether JFC: This product is resistant to acid and alkali, hard water, has good water solubility, has efficient penetration and wetting properties, and also has emulsification, dispersion and cleaning properties. It is used as a wetting agent in metal detergents to make it easy for oil stains to leave the metal surface, and also has a certain emulsification and cleaning effect.
[0015] 4. Polyepoxysuccinic acid: Polyepoxysuccinic acid (PESA) is a nitrogen-free, non-phosphorus organic compound that has both scale inhibition and corrosion inhibition effects.
[0016] 5. Disodium EDTA: It is soluble in water. It is an important chelating agent that can chelate calcium and magnesium ions in water to prevent the formation of calcium scale and magnesium scale.
[0017] 6. Polyether modified silicone defoamer: This type of defoamer is a silicone ether copolymer obtained by modifying and grafting polyether segments or polysiloxane segments. It organically combines the advantages of the two to obtain a new type of high-efficiency defoamer with the advantages of good dispersibility, strong anti-foaming ability, stability, non-toxicity, low volatility, and strong defoaming effect.
[0018] 7. Sodium hydroxide: It can react with stearic acid and oleic acid in oils and fats, and play a role in regulating pH;
[0019] 8. Isothiazolinone: Isothiazolinone is a broad-spectrum, highly effective, low-toxic, non-oxidizing biocide that can be used to kill bacteria in the system.
[0020] 9. TTA: This product is mainly used as rust inhibitor and corrosion inhibitor for copper and copper alloys.
[0021] In the above formula, it is necessary to pay attention to the dosage relationship between each substance. The dosage of each substance needs to be controlled within a reasonable range, because if the dosage of any component is too large, it will cover up the effect of other components. Although the stability is improved, the oil removal effect will be affected. Therefore, in addition to paying attention to the specific combination between the formulas, you must also pay attention to the compatibility relationship between the dosages.
[0022] The present invention also provides a method for preparing a water-soluble high-efficiency degreasing agent, comprising the following steps:
[0023] Sodium dodecylbenzene sulfonate, nonylphenol polyoxyethylene ether NP-10, and fatty alcohol polyoxyethylene ether JFC are added to the reaction kettle 1 in sequence, and stirred for 10-15 minutes until uniformly stirred to obtain a mixed solution A;
[0024] Add one-fourth of deionized water, polyepoxysuccinic acid, disodium ethylenediaminetetraacetate, and polyether-modified silicone defoamer to the reaction kettle 2 in sequence, stir for 15-20 minutes, and stir evenly to obtain a mixed solution to obtain a mixed solution B;
[0025] Add three quarters of deionized water to the reaction kettle 3, and add sodium hydroxide, isothiazolinone, and TTA in sequence while stirring. Stir for 10 minutes after each addition of a mixed solution. After stirring for 60 minutes, a mixed solution C is obtained;
[0026] Add mixed solution B and mixed solution A to mixed solution C in sequence, stirring during the addition. The stirring speed is controlled at 80-100 rpm and the temperature is controlled at 40-50°C. Stir for 0.5h each time a mixed solution is added, and finally cool to 15-30°C.
[0027] Preferably, as a further feasible solution, when preparing the mixed solution A, the stirring rate is 60-80 rpm.
[0028] Preferably, as a further feasible solution, when preparing the mixed solution B, the stirring rate is 80-120 rpm.
[0029] Preferably, as a further feasible solution, when preparing the mixed solution C, the stirring rate is 80-120 rpm.
[0030] By limiting various operating parameters in the preparation method, the quality of the prepared water-soluble high-efficiency degreasing agent is improved. The water-soluble high-efficiency degreasing agent has good stability, greatly improved degreasing rate, and can improve the descaling and sterilization effect of the degreasing agent itself.
[0031] In short, the water-soluble high-efficiency oil remover prepared by the above preparation method is green, environmentally friendly and has excellent stability.
[0032] Compared with the prior art, the beneficial effects of the above technical solution are:
[0033] (1) The degreasing agent has the characteristics of good water solubility and good degreasing effect.
[0034] (2) Degreasing agent has the function of removing scale.
[0035] (3) Degreasing agent has a bactericidal effect.
[0036] (4) Degreasing agent has the function of preventing metal corrosion.
[0037] (5) The degreasing agent will not cause phosphorus pollution to the environment.
[0038] (6) The degreasing agent preparation method is simple, easy to operate and easy to promote. DETAILED DESCRIPTION
[0039] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0040] Example 1
[0041] The specific preparation process of the water-soluble high-efficiency degreasing agent is carried out according to the following steps:
[0042] 1. Prepare each raw material according to the following mass fractions:
[0043] 8 parts of sodium dodecylbenzene sulfonate, 12 parts of nonylphenol polyoxyethylene ether NP-10, 6 parts of fatty alcohol polyoxyethylene ether JFC, 10 parts of polyepoxysuccinic acid, 5 parts of disodium ethylenediaminetetraacetic acid, 1 part of polyether modified silicone defoamer, 3 parts of sodium hydroxide, 2 parts of isothiazolinone, 0.1 parts of TTA and 10 parts of deionized water;
[0044] 2. Add sodium dodecylbenzene sulfonate, nonylphenol polyoxyethylene ether NP-10, and fatty alcohol polyoxyethylene ether JFC into the reaction kettle 1 in sequence, and stir for 10-15 minutes at 60 rpm to obtain a mixed solution A;
[0045] 3. Add one-fourth of deionized water, polyepoxysuccinic acid, disodium ethylenediaminetetraacetate, and polyether-modified silicone defoamer to reaction kettle 2 in sequence, stir for 15-20 minutes, and stir evenly at 80 rpm to obtain a mixed solution to obtain mixed solution B;
[0046] 4. Add three quarters of deionized water to the reaction kettle 3, and add sodium hydroxide, isothiazolinone, and TTA in sequence while stirring. Stir for 10 minutes after adding each mixed solution. Stir at 120 rpm for 60 minutes to obtain a mixed solution C;
[0047] 5. Add mixed solution B and mixed solution A to mixed solution C in sequence, stirring during addition. The stirring speed is controlled at 80-100 rpm and the temperature is controlled at 40-50°C. Stir for 0.5 h each time a mixed solution is added, and finally cool down to 15-30°C.
[0048] 6. After cooling to room temperature, the degreasing agent is obtained, packaged, tested, and sold as a product.
[0049] Example 2
[0050] The specific preparation process of the water-soluble high-efficiency degreasing agent is carried out according to the following steps:
[0051] 1. Prepare each raw material according to the following mass fractions:
[0052] 10 parts of sodium dodecylbenzene sulfonate, 18 parts of nonylphenol polyoxyethylene ether NP-10, 8 parts of fatty alcohol polyoxyethylene ether JFC, 14 parts of polyepoxysuccinic acid, 10 parts of disodium ethylenediaminetetraacetic acid, 3 parts of polyether modified silicone defoamer, 6 parts of sodium hydroxide, 4 parts of isothiazolinone, 0.3 parts of TTA and 20 parts of deionized water;
[0053] 2. Add sodium dodecylbenzene sulfonate, nonylphenol polyoxyethylene ether NP-10, and fatty alcohol polyoxyethylene ether JFC into the reaction kettle 1 in sequence, and stir for 10-15 minutes at 80 rpm to obtain a mixed solution A;
[0054] 3. Add one-fourth of deionized water, polyepoxysuccinic acid, disodium ethylenediaminetetraacetate, and polyether-modified silicone defoamer to reaction kettle 2 in sequence, stir for 15-20 minutes, and stir evenly at 120 rpm to obtain a mixed solution to obtain mixed solution B;
[0055] 4. Add three quarters of deionized water to the reaction kettle 3, and add sodium hydroxide, isothiazolinone, and TTA in sequence while stirring. Stir for 10 minutes after adding each mixed solution, and stir at 80 rpm for 60 minutes to obtain a mixed solution C;
[0056] 5. Add mixed solution B and mixed solution A to mixed solution C in sequence, stirring during addition. The stirring speed is controlled at 80-100 rpm and the temperature is controlled at 40-50°C. Stir for 0.5 h each time a mixed solution is added, and finally cool down to 15-30°C.
[0057] 6. After cooling to room temperature, the degreasing agent is obtained, packaged, tested, and sold as a product.
[0058] Example 3
[0059] The specific preparation process of the water-soluble high-efficiency degreasing agent is carried out according to the following steps:
[0060] 1. Prepare each raw material according to the following mass fractions:
[0061] 9 parts of sodium dodecylbenzene sulfonate, 13 parts of nonylphenol polyoxyethylene ether NP-10, 7 parts of fatty alcohol polyoxyethylene ether JFC, 11 parts of polyepoxysuccinic acid, 6 parts of disodium ethylenediaminetetraacetic acid, 2 parts of polyether modified silicone defoamer, 4 parts of sodium hydroxide, 3 parts of isothiazolinone, 0.2 parts of TTA, and 11 parts of deionized water;
[0062] 2. Add sodium dodecylbenzene sulfonate, nonylphenol polyoxyethylene ether NP-10, and fatty alcohol polyoxyethylene ether JFC into the reaction kettle 1 in sequence, and stir for 10-15 minutes at 70 rpm to obtain a mixed solution A;
[0063] 3. Add one-fourth of deionized water, polyepoxysuccinic acid, disodium ethylenediaminetetraacetate, and polyether-modified silicone defoamer to reaction kettle 2 in sequence, stir for 15-20 minutes, and stir evenly at 100 rpm to obtain a mixed solution to obtain mixed solution B;
[0064] 4. Add three quarters of deionized water to the reaction kettle 3, and add sodium hydroxide, isothiazolinone, and TTA in sequence while stirring. Stir for 10 minutes after each addition of a mixed solution. Stir at 100 rpm for 60 minutes to obtain a mixed solution C;
[0065] 5. Add mixed solution B and mixed solution A to mixed solution C in sequence, stirring during addition. The stirring speed is controlled at 80-100 rpm and the temperature is controlled at 40-50°C. Stir for 0.5 h each time a mixed solution is added, and finally cool down to 15-30°C.
[0066] 6. After cooling to room temperature, the degreasing agent is obtained, packaged, tested, and sold as a product.
[0067] Example 4
[0068] The specific preparation process of the water-soluble high-efficiency degreasing agent is carried out according to the following steps:
[0069] 1. Prepare each raw material according to the following mass fractions:
[0070] 10 parts of sodium dodecylbenzene sulfonate, 17 parts of nonylphenol polyoxyethylene ether NP-10, 8 parts of fatty alcohol polyoxyethylene ether JFC, 13 parts of polyepoxysuccinic acid, 9 parts of disodium ethylenediaminetetraacetic acid, 3 parts of polyether modified silicone defoamer, 5 parts of sodium hydroxide, 4 parts of isothiazolinone, 0.3 parts of TTA, and 19 parts of deionized water;
[0071] 2. Add sodium dodecylbenzene sulfonate, nonylphenol polyoxyethylene ether NP-10, and fatty alcohol polyoxyethylene ether JFC into the reaction kettle 1 in sequence, and stir for 10-15 minutes at 80 rpm to obtain a mixed solution A;
[0072] 3. Add one-fourth of deionized water, polyepoxysuccinic acid, disodium ethylenediaminetetraacetate, and polyether-modified silicone defoamer to reaction kettle 2 in sequence, stir for 15-20 minutes, and stir evenly at 120 rpm to obtain a mixed solution to obtain mixed solution B;
[0073] 4. Add three quarters of deionized water to the reaction kettle 3, and add sodium hydroxide, isothiazolinone, and TTA in sequence while stirring. Stir for 10 minutes after adding each mixed solution, and stir at 80 rpm for 60 minutes to obtain a mixed solution C;
[0074] 5. Add mixed solution B and mixed solution A to mixed solution C in sequence, stirring during addition. The stirring speed is controlled at 80-100 rpm and the temperature is controlled at 40-50°C. Stir for 0.5 h each time a mixed solution is added, and finally cool down to 15-30°C.
[0075] 6. After cooling to room temperature, the degreasing agent is obtained, packaged, tested, and sold as a product.
[0076] Example 5
[0077] The specific operation steps are the same as those in Example 4, except that the raw materials are prepared according to the following mass fractions:
[0078] 9 parts of sodium dodecylbenzene sulfonate, 14 parts of nonylphenol polyoxyethylene ether NP-10, 7 parts of fatty alcohol polyoxyethylene ether JFC, 11 parts of polyepoxysuccinic acid, 6 parts of disodium ethylenediaminetetraacetic acid, 2 parts of polyether modified silicone defoamer, 4 parts of sodium hydroxide, 3 parts of isothiazolinone, 0.2 parts of TTA, and 11 parts of deionized water.
[0079] Example 6
[0080] The specific operation steps are the same as those in Example 4, except that the raw materials are prepared according to the following mass fractions:
[0081] 10 parts of sodium dodecylbenzene sulfonate, 15 parts of nonylphenol polyoxyethylene ether NP-10, 8 parts of fatty alcohol polyoxyethylene ether JFC, 13 parts of polyepoxysuccinic acid, 9 parts of disodium ethylenediaminetetraacetic acid, 3 parts of polyether modified silicone defoamer, 5 parts of sodium hydroxide, 4 parts of isothiazolinone, 0.3 parts of TTA, and 19 parts of deionized water.
[0082] Comparative Example 1
[0083] The specific operation steps are the same as those in Example 4, except that the amount of sodium dodecylbenzene sulfonate added is 3 parts.
[0084] Comparative Example 2
[0085] The specific operation steps are the same as those in Example 3, except that the amount of nonylphenol polyoxyethylene ether NP-10 added is 30 parts.
[0086] Experimental Example 1
[0087] The specific treatment effects of the water-soluble high-efficiency degreasing agents of Examples 1-6 and Comparative Examples 1-2 were evaluated, and the specific results are shown in Table 1 below:
[0088] Test method and test data: Take a flat 201 stainless steel plate workpiece of the same size, spray clean it with the degreasing agent prepared in Examples 1-6 and Comparative Examples 1-2, and compare the degreasing effect.
[0089] Table 1 Experimental results
[0090] product Usage Processing temperature Processing time Treatment Effect Example 1 3% 25℃ 1 minute No oil residue Example 2 3% 25℃ 1 minute No oil residue Example 3 3% 25℃ 1 minute No oil residue Example 4 3% 25℃ 1 minute No oil residue Example 5 3% 25℃ 1 minute No oil residue Example 6 3% 25℃ 1 minute No oil residue Comparative Example 1 4% 25℃ 1.5 minutes Oil residue 15% Comparative Example 2 4% 25℃ 1.5 minutes Oil residue 15%
[0091] From the results in Table 1 above, it can be seen that the degreasing agent of the present invention removes oil thoroughly and has a strong cleaning effect. When cleaning the same stainless steel workpiece, the degreasing agent of the present invention can reduce the cleaning time by 33% and the amount used by 30%. The manufacturer can increase the cleaning output in the same time, save energy and labor, and greatly improve the production efficiency. In addition, the degreasing agent has the advantages of good water solubility, sterilization, anti-scaling, anti-corrosion and simple preparation in actual use.
[0092] Although the present invention has been illustrated and described with specific embodiments, it will be appreciated that many other changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, it is intended to include all such changes and modifications within the scope of the present invention in the appended claims.
Claims
1. A water-soluble high-efficiency degreasing agent, characterized in that: It is mainly prepared from the following raw materials: by weight: 8-10 parts of sodium dodecylbenzene sulfonate, 12-18 parts of nonylphenol polyoxyethylene ether NP-10, 6-8 parts of fatty alcohol polyoxyethylene ether JFC, 10-14 parts of polyepoxysuccinic acid, 5-10 parts of disodium ethylenediaminetetraacetic acid, 1-3 parts of polyether modified silicone defoamer, 3-6 parts of sodium hydroxide, 2-4 parts of isothiazolinone, 0.1-0.3 parts of TTA and 10-20 parts of deionized water; Sodium dodecylbenzene sulfonate, nonylphenol polyoxyethylene ether NP-10, and fatty alcohol polyoxyethylene ether JFC are added to the reaction kettle 1 in sequence, and stirred for 10-15 minutes until uniformly stirred to obtain a mixed solution A; Add one-fourth of deionized water, polyepoxysuccinic acid, disodium ethylenediaminetetraacetate, and polyether-modified silicone defoamer to the reaction kettle 2 in sequence, stir for 15-20 minutes, and stir evenly to obtain a mixed solution to obtain a mixed solution B; Add three quarters of deionized water to the reaction kettle 3, and add sodium hydroxide, isothiazolinone, and TTA in sequence while stirring. Stir for 10 minutes after each addition of a mixed solution. After stirring for 60 minutes, a mixed solution C is obtained; Add mixed solution B and mixed solution A to mixed solution C in sequence, stirring during the addition. The stirring speed is controlled at 80-100 rpm and the temperature is controlled at 40-50°C. Stir for 0.5h each time a mixed solution is added, and finally cool down to 15-30°C.
2. The water-soluble high-efficiency degreasing agent according to claim 1, characterized in that: In parts by mass, the ingredients include 9-10 parts of sodium dodecylbenzene sulfonate, 13-17 parts of nonylphenol polyoxyethylene ether NP-10, 7-8 parts of fatty alcohol polyoxyethylene ether JFC, 11-13 parts of polyepoxysuccinic acid, 6-9 parts of disodium ethylenediaminetetraacetic acid, 2-3 parts of polyether modified silicone defoamer, 4-5 parts of sodium hydroxide, 3-4 parts of isothiazolinone, 0.2-0.3 parts of TTA and 11-19 parts of deionized water.
3. The water-soluble high-efficiency degreasing agent according to claim 1, characterized in that: In parts by mass, 9 parts of sodium dodecylbenzene sulfonate, 14 parts of nonylphenol polyoxyethylene ether NP-10, 7 parts of fatty alcohol polyoxyethylene ether JFC, 11 parts of polyepoxysuccinic acid, 6 parts of disodium ethylenediaminetetraacetic acid, 2 parts of polyether modified silicone defoamer, 4 parts of sodium hydroxide, 3 parts of isothiazolinone, 0.2 parts of TTA, and 11 parts of deionized water.
4. The water-soluble high-efficiency degreasing agent according to claim 1, characterized in that: In parts by mass, 10 parts of sodium dodecylbenzene sulfonate, 15 parts of nonylphenol polyoxyethylene ether NP-10, 8 parts of fatty alcohol polyoxyethylene ether JFC, 13 parts of polyepoxysuccinic acid, 9 parts of disodium ethylenediaminetetraacetic acid, 3 parts of polyether modified silicone defoamer, 5 parts of sodium hydroxide, 4 parts of isothiazolinone, 0.3 parts of TTA, and 19 parts of deionized water.
5. The high-efficiency degreasing agent according to claim 1, characterized in that: When preparing mixed solution A, the stirring rate is 60-80 rpm.
6. The high-efficiency degreasing agent according to claim 1, characterized in that: When preparing mixed solution B, the stirring rate is 80-120 rpm.
7. The high-efficiency degreasing agent according to claim 1, characterized in that: When preparing mixed solution C, the stirring rate is 80-120 rpm.