Anion exchange membrane and its preparation method and application

Through the cross-linking reaction of polyamide epichlorohydrin and quaternary ammonium salt-modified acrylonitrile copolymer, an anion exchange membrane with high ion conductivity is prepared, which solves the carcinogenicity and cross-linking side reaction problems of the chloromethylation reaction. The preparation of environmentally friendly anion exchange membranes was realized, and the mechanical properties and industrialization potential of the membranes were improved.

CN115672047BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF -1 Cites 0 Cited by

Patent Information

Application Number
CN202110823303.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-21
Publication Date
2024-10-15
Estimated Expiration
2041-07-21

AI Technical Summary

Technical Problem

The chloromethylation reaction in the preparation of existing quaternary ammonium anionic membrane materials has carcinogenic risks and cross-linking side reactions that are difficult to control, resulting in high production costs and environmental pollution.

Method used

The anion exchange membrane is prepared through a cross-linking reaction using polyamide epichlorohydrin and acrylonitrile copolymer modified with quaternary ammonium salts. The azalated butanol structure reacts with amino groups to form an overall cross-linked membrane structure, inhibiting membrane swelling, and passing Heating and water washing treatments improve membrane performance.

Benefits of technology

It achieves the preparation of anion exchange membranes with high ion conductivity, simplifies the process, reduces environmental pollution, and improves the mechanical properties and industrial prospects of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115672047B_ABST
    Figure CN115672047B_ABST
Patent Text Reader

Abstract

The present invention provides an anion exchange membrane and a preparation method and application thereof. The anion exchange membrane is prepared from a polyamide epichlorohydrin having a structure shown in formula (I) and an acrylonitrile copolymer modified with a quaternary ammonium salt, wherein the acrylonitrile copolymer modified with a quaternary ammonium salt is prepared by reacting an acrylonitrile copolymer with a polyamine and an aldehyde compound, and then reacting with a quaternary ammonium salt containing an epoxy group. The anion exchange membrane obtained by the method has high ion conductivity, and the preparation method is simple and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer chemistry, and in particular to a preparation method and application of a composite anion exchange membrane with a cross-linked structure. Background Art

[0002] Fuel cell technology is a new energy technology that uses electrochemical reactions to convert chemical energy stored in fuels into electrical energy. Although traditional proton exchange membrane fuel cells have the advantages of high energy conversion efficiency, high energy density, and environmental friendliness, their catalysts are all relatively precious metals, and the production cost is high, which greatly limits the industrialization of batteries. In this regard, alkaline fuel cells with anion exchange membranes as electrolytes have obvious advantages, because their alkaline operating environment is conducive to improving the electrode reaction kinetics, making it possible for some non-precious metals such as Ag, Ni, Co, etc. to be used as electrocatalysts.

[0003] Anion exchange membrane is one of the key materials of alkaline fuel cells. As a solid electrolyte diaphragm, it plays a role in separating the active substances at both poles of the battery and transferring anions such as hydroxide, sulfate or halogen. Looking at the relevant literature and patents at home and abroad, quaternary ammonium anion membrane is still the main body of anion membrane. The preparation of quaternary ammonium anion membrane materials often requires chloromethylation, and the most commonly used chloromethylation agent (chloromethyl methyl ether) has strong carcinogenicity. In addition, the chloromethylation position during the chloromethylation reaction is difficult to accurately control, and cross-linking side reactions are prone to occur.

[0004] Therefore, it is of great significance to develop anion exchange membrane materials that are simple in preparation and environmentally friendly. Summary of the invention

[0005] The purpose of the present invention is to provide an anion exchange membrane and a preparation method and application thereof. The anion exchange membrane obtained by the method has high ion conductivity, and the preparation method is simple and environmentally friendly.

[0006] One of the purposes of the present invention is to provide an anion exchange membrane prepared from a copolymer of polyamide epichlorohydrin and quaternary ammonium salt-modified acrylonitrile having a structure shown in formula (I).

[0007]

[0008] Preferably, the mass ratio of the polyamide epichlorohydrin to the quaternary ammonium salt-modified acrylonitrile copolymer is (0.1-100):1, more preferably (0.5-50):1.

[0009] Preferably, the thickness of the anion exchange membrane is 10 to 100 μm, more preferably 30 to 60 μm.

[0010] The quaternary ammonium salt-modified acrylonitrile copolymer is prepared by reacting the acrylonitrile copolymer with polyamine and aldehyde compounds, and then reacting with a quaternary ammonium salt containing an epoxy group.

[0011] The acrylonitrile copolymer is selected from at least one of polyacrylonitrile, styrene-acrylonitrile copolymer, acrylonitrile-butadiene-styrene copolymer, methyl methacrylate-acrylonitrile copolymer, butadiene-acrylonitrile copolymer, acrylonitrile-methacrylonitrile copolymer, acrylate-acrylonitrile copolymer and ethylene-propylene-styrene-acrylonitrile copolymer.

[0012] The polyamine is selected from at least one of 1,3,5-triaminobenzene, melamine, diethylenetriamine, tetraethylenepentamine, polyethyleneimine, polyethylenepolyamine and polyetheramine.

[0013] The aldehyde compound is selected from at least one of formaldehyde, acetaldehyde, propionaldehyde, n-butyraldehyde, n-valeraldehyde, benzaldehyde, n-heptylaldehyde and paraformaldehyde.

[0014] The epoxy group-containing quaternary ammonium salt is selected from ammonium halides, preferably at least one selected from 2,3-epoxypropyltrimethylammonium chloride, 2,3-epoxypropyltriethylammonium chloride, 1,2-epoxypropyldimethyldodecylammonium chloride, diethyl-2,3-epoxypropyl-[3-(methyldimethoxy)]silylpropylammonium chloride, 2,3-epoxypropyltrimethylammonium bromide, 2,3-epoxypropyltriethylammonium bromide, 1,2-epoxypropyldimethyldodecylammonium bromide, and diethyl-2,3-epoxypropyl-[3-(methyldimethoxy)]silylpropylammonium bromide.

[0015] The second object of the present invention is to provide a method for preparing the anion exchange membrane, comprising dispersing a quaternary ammonium salt-modified acrylonitrile copolymer into a polyamide epichlorohydrin solution to obtain a casting solution, scraping the membrane, and heating to obtain a membrane; then immersing the obtained membrane in an aqueous solution of sodium hydroxide and / or potassium hydroxide, and washing with water to obtain the anion exchange membrane.

[0016] In the preparation method of the present invention, the polyamide epichlorohydrin has a structure shown in formula (I).

[0017] In the preparation method of the present invention, the mass ratio of the polyamide epichlorohydrin to the quaternary ammonium salt modified acrylonitrile copolymer is (0.1-100):1, more preferably (0.5-50):1.

[0018] In the preparation method of the present invention, based on 100 parts of the casting solution, the content of polyamide epichlorohydrin is 1 to 20 parts, preferably 2 to 10 parts; the content of quaternary ammonium salt modified acrylonitrile copolymer is 0.01 to 10 parts, preferably 0.1 to 5 parts.

[0019] In the preparation method of the present invention, the heating temperature is 40 to 150° C., preferably 80 to 120° C.; the heating time is 1 to 30 minutes, preferably 5 to 15 minutes.

[0020] In the preparation method of the present invention, the content of sodium hydroxide and / or potassium hydroxide in the aqueous solution of sodium hydroxide and / or potassium hydroxide is 0.5-10wt%, preferably 1-5wt%.

[0021] In the preparation method of the present invention, the time for soaking the membrane in the aqueous solution is 10 to 36 hours, preferably 20 to 30 hours.

[0022] In the preparation method of the present invention, the quaternary ammonium salt-modified acrylonitrile copolymer is prepared by the following steps:

[0023] (a) dispersing an acrylonitrile copolymer in a solution containing a polyamine and an aldehyde compound, heating the solution to react, and obtaining an amino-modified acrylonitrile copolymer; (b) adding the amino-modified acrylonitrile copolymer obtained in step (a) to a solution of a quaternary ammonium salt containing an epoxy group, heating the solution to react, and obtaining an acrylonitrile copolymer modified with a quaternary ammonium salt.

[0024] In the above step (a), the mass concentration of the acrylonitrile copolymer is 0.5 to 20 parts, preferably 1 to 10 parts, based on 100 parts of the solution; the mass concentration of the polyamine is 0.5 to 10 parts, preferably 1 to 5 parts, based on 100 parts of the solution; the mass concentration of the aldehyde compound is 0.1 to 5 parts, preferably 0.5 to 2.5 parts, based on 100 parts of the solution.

[0025] In the above step (a), the reaction time is 1 to 24 hours, preferably 3 to 12 hours; the reaction temperature is 25 to 100°C, preferably 50 to 80°C.

[0026] In the above step (b), the mass concentration of the quaternary ammonium salt containing epoxy groups is 1 to 20 parts, preferably 2 to 10 parts, and more preferably 2 to 5 parts, based on 100 parts of the solution.

[0027] In the above step (b), the mass ratio of the amino-modified acrylonitrile copolymer to the quaternary ammonium salt containing epoxy groups is (0.01-20):1, preferably (0.1-10):1.

[0028] In the above step (b), the reaction temperature is 20 to 80° C., preferably 25 to 40° C.; the reaction time is 1 to 12 h, preferably 2 to 6 h.

[0029] The third object of the present invention is to provide an anion exchange membrane obtained by the preparation method.

[0030] A fourth object of the present invention is to provide applications of the composite anion exchange membrane and the anion exchange membrane obtained by the preparation method in the field of fuel cells.

[0031] The inventors of the present invention have found through in-depth research that the hydroxyl group in the azetidinol structure in the polyamide epichlorohydrin molecular chain can react with the amino group of the polyamide epichlorohydrin and the amino group in the acrylonitrile copolymer modified with a quaternary ammonium salt. The former reaction can form an overall cross-linked membrane structure to inhibit the swelling of the membrane; the latter cross-linking reaction can make the acrylonitrile copolymer micron powder modified with a quaternary ammonium salt more compatible in the membrane, avoid the occurrence of phase separation, and improve the mechanical properties of the membrane.

[0032] In addition, the preparation method of the present invention has simple process, is green and environmentally friendly, and has great industrial prospects.

[0033] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is the infrared spectrum of polyacrylonitrile (PAN) and polyacrylonitrile modified with epoxy quaternary ammonium salt (PAN-NH4Cl). DETAILED DESCRIPTION

[0035] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.

[0036] The invention provides an anion exchange membrane, which is formed by cross-linking polyamide epichlorohydrin having a structure shown in formula (I) and acrylonitrile copolymer micron powder modified by quaternary ammonium salt, wherein the acrylonitrile copolymer micron powder modified by quaternary ammonium salt is prepared by reacting acrylonitrile copolymer micron powder with polyamine, aldehyde compound and quaternary ammonium salt containing epoxy group.

[0037]

[0038] The present invention has no special limitation on the thickness of the anion exchange membrane, which may be a conventional choice in the art. However, in order to make the obtained anion exchange membrane have better ion conductivity and fuel permeation barrier properties, according to a preferred embodiment of the present invention, the membrane thickness is 10 to 100 μm, preferably 30 to 60 μm.

[0039] According to a preferred embodiment of the present invention, the mass ratio of the polyamide epichlorohydrin to the quaternary ammonium salt modified acrylonitrile copolymer micron powder is (0.1-100):1, more preferably (0.5-50):1, and further preferably (0.5-25):1.

[0040] The present invention also provides a method for preparing an anion exchange membrane, comprising dispersing a quaternary ammonium salt-modified acrylonitrile copolymer into a polyamide epichlorohydrin solution to obtain a membrane casting solution, scraping the membrane, and heating to obtain a membrane; then immersing the obtained membrane in an aqueous solution of sodium hydroxide and / or potassium hydroxide, and washing with water to obtain the anion exchange membrane.

[0041] The quaternary ammonium salt modified acrylonitrile copolymer is prepared by the following steps: (a) dispersing the acrylonitrile copolymer in a solution containing polyamine and aldehyde compound, heating for reaction, and obtaining an amino-modified acrylonitrile copolymer; (b) adding the amino-modified acrylonitrile copolymer obtained in step (a) into a solution of quaternary ammonium salt containing epoxy group, heating for reaction, and obtaining a quaternary ammonium salt modified acrylonitrile copolymer.

[0042] According to a preferred embodiment of the present invention, the method may include the following steps: (1) dispersing acrylonitrile copolymer powder into a solution containing polyamine and aldehyde compound, uniformly dispersing by ultrasonication, and heating under stirring for reaction; filtering and rinsing with deionized water to obtain amino-modified acrylonitrile copolymer powder; (2) adding the polymer powder obtained in step (1) into a solution containing epoxy ammonium salt, heating for reaction, filtering and rinsing with deionized water to obtain quaternary ammonium salt-modified acrylonitrile copolymer powder; (3) dispersing the polymer powder obtained in step (2) into a polyamide epichlorohydrin solution, uniformly dispersing by ultrasonication, pouring the solution onto a clean glass plate, heating and drying to obtain a membrane material; and (4) immersing the obtained membrane in an aqueous sodium hydroxide solution, and washing with water to obtain an anion exchange membrane.

[0043] According to a preferred embodiment of the present invention, in the step (1), the acrylonitrile copolymer is one or a mixture of polyacrylonitrile, styrene-acrylonitrile copolymer, acrylonitrile-butadiene-styrene copolymer, methyl methacrylate-acrylonitrile copolymer, butadiene-acrylonitrile copolymer, acrylonitrile-methacrylonitrile copolymer, acrylate-acrylonitrile copolymer, ethylene-propylene-styrene-acrylonitrile copolymer.

[0044] According to a preferred embodiment of the present invention, in the step (1), the polyamine is one or a mixture of 1,3,5-triaminobenzene, melamine, diethylenetriamine, tetraethylenepentamine, polyethyleneimine, polyethylenepolyamine and polyetheramine, preferably polyethyleneimine and polyethylenepolyamine; the aldehyde compound is one or a mixture of formaldehyde, acetaldehyde, propionaldehyde, n-butyraldehyde, n-valeraldehyde, n-heptylaldehyde, benzaldehyde and paraformaldehyde.

[0045] According to a preferred embodiment of the present invention, in the step (1), the content of acrylonitrile copolymer is 0.5 to 20 parts, preferably 1 to 10 parts, based on 100 parts of the solution; the mass concentration of the polyamine is 0.5 to 10 parts, preferably 1 to 5 parts, based on 100 parts of the solution; the mass concentration of the aldehyde compound is 0.1 to 5 parts, preferably 0.5 to 2.5 parts, based on 100 parts of the solution.

[0046] According to a preferred embodiment of the present invention, in the step (1), the reaction time is 1 to 24 hours, preferably 3 to 12 hours; the reaction temperature is 25 to 100°C, preferably 50 to 80°C.

[0047] According to a preferred embodiment of the present invention, in the step (2), the quaternary ammonium salt containing an epoxy group is selected from one or more of 2,3-epoxypropyltrimethylammonium chloride, 2,3-epoxypropyltriethylammonium chloride, 1,2-epoxypropyldimethyldodecylammonium chloride, diethyl-2,3-epoxypropyl-[3-(methyldimethoxy)]silylpropylammonium chloride, 2,3-epoxypropyltrimethylammonium bromide, 2,3-epoxypropyltriethylammonium bromide, 1,2-epoxypropyldimethyldodecylammonium bromide and diethyl-2,3-epoxypropyl-[3-(methyldimethoxy)]silylpropylammonium bromide.

[0048] According to a preferred embodiment of the present invention, in the step (2), there is no special limitation on the mass concentration of the quaternary ammonium salt containing epoxy groups. However, in order to make the obtained anion exchange membrane have better ion conductivity and fuel permeation barrier properties, preferably, the content of the quaternary ammonium salt containing epoxy groups is 1 to 20 parts, preferably 2 to 10 parts, and more preferably 2 to 5 parts, based on 100 parts of the solution.

[0049] According to a preferred embodiment of the present invention, in the step (2), the mass ratio of the amino-modified acrylonitrile copolymer powder to the epoxy group-containing quaternary ammonium salt is (0.01-20):1, preferably (0.1-10):1.

[0050] According to a preferred embodiment of the present invention, in the step (2), there is no special limitation on the reaction conditions, but in order to make the obtained anion exchange membrane have better ion conductivity and fuel permeation barrier, preferably, the reaction temperature is 20 to 80°C, preferably 25 to 40°C; the reaction time is 1 to 12 hours, preferably 2 to 6 hours.

[0051] According to a preferred embodiment of the present invention, in the step (3), the mass ratio of the polyamide epichlorohydrin to the quaternary ammonium salt modified acrylonitrile copolymer is (0.1-100):1, more preferably (0.5-50):1. There is no particular limitation on the mass concentration of the polyamide epichlorohydrin and quaternary ammonium salt modified acrylonitrile copolymer powders, but in order to make the obtained anion exchange membrane have better ion conductivity and fuel permeation barrier, preferably, the mass concentration of the polyamide epichlorohydrin and quaternary ammonium salt modified acrylonitrile copolymer powders is 1-20 parts, preferably 2-10 parts, based on 100 parts of the solution; the content of the quaternary ammonium salt modified acrylonitrile copolymer powder is 0.01-10 parts, preferably 0.1-5 parts.

[0052] According to a preferred embodiment of the present invention, in the step (3), there is no special limitation on the heating treatment conditions. However, in order to enable the obtained anion exchange membrane to have better ion conductivity and fuel permeation barrier properties, preferably, the heating temperature is 40 to 150°C, preferably 80 to 120°C; the heating time is 1 min to 30 min, preferably 5 min to 15 min.

[0053] According to a preferred embodiment of the present invention, in step (4), there is no special limitation on the concentration of the sodium hydroxide. In order to make the obtained anion exchange membrane have better ion conductivity and fuel permeation barrier, preferably, the content of sodium hydroxide is 0.5 to 10 wt%, preferably 1 to 5 wt%.

[0054] According to a preferred embodiment of the present invention, in the step (4), there is no special limitation on the time for soaking the membrane in the sodium hydroxide aqueous solution. However, in order to enable the obtained anion exchange membrane to have better ion conductivity and fuel permeation barrier properties, the soaking time is preferably 10 h to 36 h, preferably 20 h to 30 h.

[0055] According to a preferred embodiment of the present invention, in steps (1), (2) and (3), the solvent of the solution is selected from one or more of water, methanol, ethanol and the like.

[0056] The reaction mechanism of the quaternary ammonium salt-modified acrylonitrile copolymer in one embodiment of the preparation of the anion exchange membrane is given below:

[0057]

[0058] The reaction mechanism of polyamide epichlorohydrin soaked in NaOH in one embodiment of the preparation of the anion exchange membrane is given below:

[0059]

[0060] In the following examples and comparative examples:

[0061] (1) Proton conductivity test: The proton conductivity was measured by AC impedance spectroscopy (Salton 1260) using the four-electrode method. The proton conductivity was calculated using the following formula: σ = L / RS, where L is the distance between the electrodes (cm); S is the cross-sectional area of ​​the membrane (cm 2 ), R is the resistance of the membrane (Ω).

[0062] (2) Test of water absorption and swelling rate of membrane: Soak the membrane in 80℃ distilled water for 24h and then take it out. Quickly wipe off the water on the membrane surface, weigh it and measure the size of the membrane. Water absorption and swelling rate are the percentage changes in mass and size of the membrane after absorbing water to saturation.

[0063] (3) Methanol permeability test: 150 mL of high-purity water and an equal amount of methanol solution (10 M) were placed in the two half-cells A and B of the stainless steel diffusion cell, and the two half-cells were separated by a polymer membrane. After magnetic stirring for several hours, the liquid on the high-purity water side was taken out and the methanol concentration was measured using a SHIMADZU GC-8A gas chromatograph. The methanol permeability was calculated by the following formula:

[0064]

[0065] Among them, C A :Methanol concentration in pool A (10 mol L -1 ), C B :Methanol concentration in pool B (mol L -1 ), V B : Volume of methanol solution in pool B (L), P: methanol permeability (cm 2 s -1 ), A: the opening area between pool A and pool B (cm 2 ), L is the film thickness (cm).

[0066] (4) Film Thickness The cross-sectional morphology of the film was observed using a Hitachi S-4800 high-resolution field emission scanning electron microscope (FESEM) to obtain the film thickness.

[0067] (5) The molecular structure of the membrane surface was measured by infrared spectrometer (ATR-FTIR) (Nicolet 6700).

[0068] In addition, in the following examples and comparative examples:

[0069] Polyacrylonitrile was purchased from McLean (number average molecular weight of 80,000), acrylonitrile-styrene copolymer, branched polyethyleneimine (weight average molecular weight of 25,000), polyethylene polyamine, diethylenetriamine, tetraethylenepentamine, 2,3-epoxypropyltrimethylammonium chloride, 2,3-epoxypropyltriethylammonium chloride, 1,2-epoxypropyldimethyldodecylammonium chloride, 2,3-epoxypropyltrimethylammonium bromide, etc. were all purchased from J&K Technology Co., Ltd., polyamide polyamine epichlorohydrin was purchased from China Pulp and Paper Research Institute Co., Ltd., and other chemical reagents were purchased from Sinopharm Chemical Reagent Co., Ltd.

[0070] Preparation Example 1

[0071] 1 g of polyacrylonitrile powder was dispersed in 100 g of an aqueous solution containing 1 wt % polyethyleneimine and 0.5 wt % formaldehyde, reacted at 60° C. for 3 h, filtered, and repeatedly rinsed with deionized water to obtain an amino-modified polyacrylonitrile powder; then, 10 g of the powder was dispersed in 100 g of an aqueous solution containing 5 wt % 2,3-epoxypropyltrimethylammonium chloride, reacted at 40° C. for 6 h, filtered, repeatedly rinsed with deionized water, and dried to obtain a quaternary ammonium salt-modified polyacrylonitrile powder.

[0072] Figure 1 This is the infrared spectrum of polyacrylonitrile (PAN) and 2,3-epoxypropyltrimethylammonium chloride modified polyacrylonitrile powder (PAN-NH4Cl). Figure 1 It can be seen that after PAN powder modification, the -1 and 3389cm -1 New absorption peaks appeared at 40°, corresponding to the ammonium chloride group and the hydroxyl group generated after the epoxy ring opening, respectively. This proves that the ammonium chloride group was successfully modified to PAN powder through the two-step modification method.

[0073] Preparation Example 2

[0074] 10 g of polyacrylonitrile powder was dispersed in 100 g of an aqueous solution containing 5 wt % polyethyleneimine and 2.5 wt % formaldehyde, reacted at 60° C. for 3 h, filtered, and repeatedly rinsed with deionized water to obtain an amino-modified polyacrylonitrile powder; then, 5 g of the powder was dispersed in 100 g of an aqueous solution containing 5 wt % 2,3-epoxypropyltrimethylammonium chloride, reacted at 40° C. for 6 h, filtered, repeatedly rinsed with deionized water, and dried to obtain a quaternary ammonium salt-modified polyacrylonitrile powder.

[0075] Preparation Example 3

[0076] The method is the same as that of Preparation Example 1, except that polyethylene imine is replaced by polyethylene polyamine, and 2,3-epoxypropyltriethylammonium chloride is replaced by 2,3-epoxypropyltrimethylammonium chloride to obtain quaternary ammonium salt-modified polyacrylonitrile powder.

[0077] Preparation Example 4

[0078] The method is the same as that of Preparation Example 1, except that diethylenetriamine is used instead of polyethyleneimine, and 1,2-epoxypropyldimethyldodecylammonium chloride is used instead of 2,3-epoxypropyltrimethylammonium chloride to obtain quaternary ammonium salt-modified polyacrylonitrile powder.

[0079] Preparation Example 5

[0080] The method is the same as that of Preparation Example 1, except that tetraethylenepentamine is used instead of polyethyleneimine, and 2,3-epoxypropyltrimethylammonium bromide is used instead of 2,3-epoxypropyltrimethylammonium chloride to obtain quaternary ammonium salt-modified polyacrylonitrile powder.

[0081] Preparation Example 6

[0082] The method is the same as that of Preparation Example 1, except that acrylonitrile-styrene copolymer is used instead of polyacrylonitrile to obtain quaternary ammonium salt-modified acrylonitrile-styrene copolymer powder.

[0083] Preparation Example 7

[0084] 1 g of polyacrylonitrile powder was dispersed in 100 g of an aqueous solution containing 1 wt % polyethyleneimine and 0.5 wt % formaldehyde, and reacted at 60° C. for 3 h. The resulting amino-modified polyacrylonitrile powder was filtered and repeatedly rinsed with deionized water.

[0085] Example 1

[0086] 0.2 g of the quaternary ammonium salt-modified polyacrylonitrile powder obtained in Preparation Example 1 was dispersed in 10 g of a polyamide polyamine epichlorohydrin aqueous solution with a mass concentration of 5 wt %. After ultrasonic dispersion, the dispersion was poured onto a clean glass plate and heated at 120° C. for 10 min to obtain a membrane material. Finally, the obtained membrane material was immersed in a 4 wt % NaOH aqueous solution for 24 h, taken out, and rinsed with deionized water until neutral to obtain an anion exchange membrane N1 with a membrane thickness of 35 μm.

[0087] The obtained composite anion exchange membrane N1 was immersed in 80°C water for 24h, and the water absorption and swelling rate of the membrane were tested. The results are shown in Table 1. The hydroxide conductivity of the membrane in 80°C water and the methanol permeability at room temperature are also shown in Table 1.

[0088] Example 2

[0089] 0.05 g of the quaternary ammonium salt-modified polyacrylonitrile powder obtained in Preparation Example 2 was dispersed in 10 g of a 10 wt % polyamide polyamine epichlorohydrin aqueous solution, and after ultrasonic dispersion, the dispersion was poured onto a clean glass plate and heated at 80° C. for 15 min to obtain a membrane material; finally, the obtained membrane material was immersed in a 4 wt % NaOH aqueous solution for 24 h, taken out, and rinsed with deionized water until neutral to obtain an anion exchange membrane N2 with a membrane thickness of 42 μm.

[0090] The obtained composite anion exchange membrane N2 was immersed in 80°C water for 24h, and the water absorption and swelling rate of the membrane were tested. The results are shown in Table 1. The hydroxide conductivity of the membrane in 80°C water and the methanol permeability at room temperature are also shown in Table 1.

[0091] Example 3

[0092] 0.5 g of the quaternary ammonium salt-modified polyacrylonitrile powder obtained in Preparation Example 3 was dispersed in 10 g of a polyamide polyamine epichlorohydrin aqueous solution with a mass concentration of 2.5 wt %. After ultrasonic dispersion, the dispersion was poured onto a clean glass plate and heated at 100° C. for 15 min to obtain a membrane material. Finally, the obtained membrane material was immersed in a 4 wt % NaOH aqueous solution for 24 h, taken out, and rinsed with deionized water until neutral to obtain an anion exchange membrane N3 with a membrane thickness of 29 μm.

[0093] The obtained composite anion exchange membrane N3 was immersed in 80°C water for 24h, and the water absorption rate and swelling rate of the membrane were tested. The results are shown in Table 1. The hydroxide conductivity of the membrane in 80°C water and the methanol permeability at room temperature are also shown in Table 1.

[0094] Example 4

[0095] According to the method of Example 1, except that the quaternary ammonium salt-modified polyacrylonitrile powder obtained in Preparation Example 4 was used instead of the quaternary ammonium salt-modified polyacrylonitrile powder obtained in Preparation Example 1, an anion exchange membrane N4 was prepared, and the membrane thickness was 37 μm.

[0096] The obtained composite anion exchange membrane N4 was immersed in 80°C water for 24h, and the water absorption and swelling rate of the membrane were tested. The results are shown in Table 1. The hydroxide conductivity of the membrane in 80°C water and the methanol permeability at room temperature are also shown in Table 1.

[0097] Example 5

[0098] An anion exchange membrane N5 was prepared according to the method of Example 1, except that the quaternary ammonium salt-modified polyacrylonitrile powder obtained in Preparation Example 5 was used instead of the quaternary ammonium salt-modified polyacrylonitrile powder obtained in Preparation Example 1. The thickness of the membrane was 34 μm.

[0099] The obtained composite anion exchange membrane N5 was immersed in 80°C water for 24 hours, and the water absorption rate and swelling rate of the membrane were tested. The results are shown in Table 1. The hydroxide conductivity of the membrane in 80°C water and the methanol permeability at room temperature are also shown in Table 1.

[0100] Example 6

[0101] An anion exchange membrane N6 was prepared according to the method of Example 1, except that the quaternary ammonium salt-modified acrylonitrile-styrene copolymer powder obtained in Preparation Example 6 was used instead of the quaternary ammonium salt-modified polyacrylonitrile powder obtained in Preparation Example 1. The thickness of the membrane was 29 μm.

[0102] The obtained composite anion exchange membrane N6 was immersed in 80°C water for 24 hours, and the water absorption and swelling rate of the membrane were tested. The results are shown in Table 1. The hydroxide conductivity of the membrane in 80°C water and the methanol permeability at room temperature are also shown in Table 1.

[0103] Comparative Example 1

[0104] The method of Example 1 was followed, except that unmodified polyacrylonitrile powder was used instead of the polyacrylonitrile powder modified with quaternary ammonium salt obtained in Preparation Example 1 to prepare an anion exchange membrane D1, the thickness of which was 33 μm.

[0105] The obtained composite anion exchange membrane D1 was immersed in 80°C water for 24h, and the water absorption and swelling rate of the membrane were tested. The results are shown in Table 1. The hydroxide conductivity of the membrane in 80°C water and the methanol permeability at room temperature are also shown in Table 1.

[0106] Comparative Example 2

[0107] An anion exchange membrane D2 was prepared according to the method of Example 1, except that the amino-modified polyacrylonitrile powder obtained in Preparation Example 7 was used instead of the quaternary ammonium salt-modified polyacrylonitrile powder obtained in Preparation Example 1. The thickness of the membrane was 35 μm.

[0108] The obtained composite anion exchange membrane D2 was immersed in 80°C water for 24 hours, and the water absorption rate and swelling rate of the membrane were tested. The results are shown in Table 1. The hydroxide conductivity of the membrane in 80°C water and the methanol permeability at room temperature are also shown in Table 1.

[0109] Comparative Example 3

[0110] The method of Example 1 is followed, except that the casting solution contains only polyamide polyamine epichlorohydrin. After film laying and drying, an anion exchange membrane D3 is obtained, and the thickness of the membrane is 30 μm.

[0111] The obtained composite anion exchange membrane D3 was immersed in 80°C water for 24h, and the water absorption and swelling rate of the membrane were tested. The results are shown in Table 1. The hydroxide conductivity of the membrane in 80°C water and the methanol permeability at room temperature are also shown in Table 1.

[0112] Table 1

[0113]

[0114] As can be seen from Table 1, the hydroxyl group in the azidobutanol structure in the polyamide epichlorohydrin molecular chain can react with the amino group in the polyacrylonitrile modified with quaternary ammonium salt to form a cross-linked structure, thereby inhibiting the swelling of the membrane and improving the alcohol resistance of the membrane. On the other hand, the cross-linking between polyamide epichlorohydrin and modified polyacrylonitrile can make the powder more compatible in the membrane, avoid the occurrence of phase separation, and improve the mechanical properties of the membrane; in addition, the introduction of quaternary ammonium salt modified polyacrylonitrile increases the content of quaternary ammonium groups in the membrane, which helps to improve the conductivity of the membrane to hydroxide ions.

Claims

1. An anion exchange membrane prepared from a copolymer of polyamide epichlorohydrin and quaternary ammonium salt-modified acrylonitrile having a structure represented by formula (I), (I); The mass ratio of the polyamide epichlorohydrin to the quaternary ammonium salt-modified acrylonitrile copolymer is (0.1-100):1; the quaternary ammonium salt-modified acrylonitrile copolymer is prepared by reacting an acrylonitrile copolymer with a polyamine and an aldehyde compound, and then reacting with a quaternary ammonium salt containing an epoxy group; the quaternary ammonium salt containing an epoxy group is selected from at least one of 2,3-epoxypropyltrimethylammonium chloride, 2,3-epoxypropyltriethylammonium chloride, 1,2-epoxypropyldimethyldodecylammonium chloride, diethyl-2,3-epoxypropyl-[3-(methyldimethoxy)]silylpropylammonium chloride, 2,3-epoxypropyltrimethylammonium bromide, 2,3-epoxypropyltriethylammonium bromide, 1,2-epoxypropyldimethyldodecylammonium bromide and diethyl-2,3-epoxypropyl-[3-(methyldimethoxy)]silylpropylammonium bromide.

2. The anion exchange membrane according to claim 1, characterized in that: The mass ratio of the polyamide epichlorohydrin to the quaternary ammonium salt modified acrylonitrile copolymer is (0.5-50):1; and / or, The thickness of the anion exchange membrane is 10-100 μm.

3. The anion exchange membrane according to claim 2, characterized in that: The thickness of the anion exchange membrane is 30-60 μm.

4. The anion exchange membrane according to claim 1, characterized in that: The acrylonitrile copolymer is selected from at least one of polyacrylonitrile, styrene-acrylonitrile copolymer, acrylonitrile-butadiene-styrene copolymer, methyl methacrylate-acrylonitrile copolymer, butadiene-acrylonitrile copolymer, acrylonitrile-methacrylonitrile copolymer, acrylate-acrylonitrile copolymer and ethylene-propylene-styrene-acrylonitrile copolymer; and / or, The polyamine is selected from at least one of 1,3,5-triaminobenzene, melamine, diethylenetriamine, tetraethylenepentamine, polyethyleneimine, polyethylenepolyamine and polyetheramine; and / or, The aldehyde compound is selected from at least one of formaldehyde, acetaldehyde, propionaldehyde, n-butyraldehyde, n-valeraldehyde, benzaldehyde, n-heptylaldehyde and paraformaldehyde.

5. A method for preparing an anion exchange membrane according to any one of claims 1 to 4, comprising dispersing a quaternary ammonium salt-modified acrylonitrile copolymer into a polyamide epichlorohydrin solution to obtain a casting solution, scraping the film, and heating to obtain a membrane; then immersing the obtained membrane in an aqueous solution of sodium hydroxide and / or potassium hydroxide, and washing with water to obtain the anion exchange membrane.

6. The preparation method according to claim 5, characterized in that: Based on 100 parts of the casting solution, the content of polyamide epichlorohydrin is 1 to 20 parts; the content of quaternary ammonium salt-modified acrylonitrile copolymer is 0.01 to 10 parts; and / or, The heating temperature is 40~150℃; the heating time is 1~30min.

7. The preparation method according to claim 6, characterized in that: Based on 100 parts of the casting solution, the content of polyamide epichlorohydrin is 2 to 10 parts; the content of quaternary ammonium salt-modified acrylonitrile copolymer is 0.1 to 5 parts; and / or, The heating temperature is 80~120℃; the heating time is 5~15min.

8. The preparation method according to claim 5, characterized in that: The aqueous solution of sodium hydroxide and / or potassium hydroxide has a content of 0.5 to 10 wt % of sodium hydroxide and / or potassium hydroxide; and / or, The time for soaking the membrane in the aqueous solution is 10 to 36 hours.

9. The preparation method according to claim 8, characterized in that: The aqueous solution of sodium hydroxide and / or potassium hydroxide has a content of 1 to 5 wt %; and / or, The time for soaking the membrane in the aqueous solution is 20 to 30 hours.

10. The preparation method according to claim 5, characterized in that The quaternary ammonium salt-modified acrylonitrile copolymer is prepared by the following steps: (a) dispersing an acrylonitrile copolymer in a solution containing a polyamine and an aldehyde compound, heating the solution to react, and obtaining an amino-modified acrylonitrile copolymer; (b) adding the amino-modified acrylonitrile copolymer obtained in step (a) to a solution of a quaternary ammonium salt containing an epoxy group, heating the solution to react, and obtaining an acrylonitrile copolymer modified with a quaternary ammonium salt.

11. The preparation method according to claim 10, characterized in that In the step (a): Based on 100 parts of the solution, the content of acrylonitrile copolymer is 0.5 to 20 parts; based on 100 parts of the solution, the content of polyamine is 0.5 to 10 parts; based on 100 parts of the solution, the content of aldehyde compound is 0.1 to 5 parts; and / or, The reaction time is 1~24h; the reaction temperature is 25~100℃.

12. The preparation method according to claim 11, characterized in that: Based on 100 parts of the solution, the content of acrylonitrile copolymer is 1 to 10 parts; based on 100 parts of the solution, the content of polyamine is 1 to 5 parts; based on 100 parts of the solution, the content of aldehyde compound is 0.5 to 2.5 parts; and / or, The reaction time is 3~12h; the reaction temperature is 50~80℃.

13. The preparation method according to claim 10, characterized in that In the step (b): Based on 100 parts of the solution, the content of the quaternary ammonium salt containing epoxy groups is 1 to 20 parts; and / or, The mass ratio of the amino-modified acrylonitrile copolymer to the epoxy-group-containing quaternary ammonium salt is (0.01-20):1; and / or, The reaction temperature is 20~80℃; the reaction time is 1~12h.

14. The preparation method according to claim 13, characterized in that: Based on 100 parts of the solution, the content of the quaternary ammonium salt containing epoxy groups is 2 to 10 parts; and / or, The mass ratio of the amino-modified acrylonitrile copolymer to the quaternary ammonium salt containing an epoxy group is (0.1-10):1 and / or, The reaction temperature is 25~40℃; the reaction time is 2~6h.

15. An anion exchange membrane obtained according to the preparation method according to any one of claims 5 to 14.

16. Use of the anion exchange membrane according to any one of claims 1 to 4 and the anion exchange membrane obtained by the preparation method according to any one of claims 5 to 14 in a fuel cell.