Acrylamide copolymer and its preparation method and application
By introducing acrylamide copolymers with superhydrophilic groups and sulfonic acid groups into the polymer, the problem of degradation of oil-driving effect under high temperature and high salt conditions is solved, high viscosity and low oil-water meter interface tension are achieved, and oil is improved The effect of hiding the depth is adjusted and driven.
Patent Information
- Application Number
- CN202110857672.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-07-28
AI Technical Summary
The existing polymer oil flooding technology has shown a significant reduction in oil flooding effect under high temperature and high salt conditions, and cannot effectively enter the deep reservoir, resulting in low recovery and poor effect.
Using acrylamide copolymers containing structural units A, B and C, the temperature resistance and salt resistance of the copolymer are improved and emulsified by introducing monomers of superhydrophilic groups and sulfonic acid groups in the polymerization reaction, thereby enhancing the temperature resistance and salt resistance of the copolymer. Viscosity and emulsification capacity under high temperature and high salt conditions.
It achieves high viscosity and low oil-water meter interface tension under high temperature (100℃) and high mineralization (48000mg/L), which can effectively enter the deep reservoir and improve the deep driving effect.
Smart Images

Figure CN115677917B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of oilfield chemicals, and in particular to an acrylamide copolymer and a preparation method and application thereof. Background Art
[0002] In tertiary oil recovery, the use of water-soluble polymer flooding has developed into an extremely important technology for improving oil recovery. Water-soluble polymers have good water solubility and viscosity-increasing properties. When they are added to water, the viscosity of the aqueous solution can be significantly increased, the water / oil mobility ratio under the reservoir can be reduced, and the fluid swept volume and sweep efficiency can be increased, and the oil saturation in the swept area can be reduced, thereby achieving the purpose of improving oil recovery. The results of the field implementation in the oil field show that the use of polymer flooding can greatly improve the crude oil recovery rate and produce huge economic and social benefits. At present, the polymer used in polymer flooding is mainly partially hydrolyzed polyacrylamide, which has excellent viscosity-increasing properties under conventional reservoir conditions and shows good oil recovery effect, but the oil recovery effect is significantly reduced under high temperature and high salt conditions. This is because the polymer molecular chain will curl and degrade rapidly under high temperature and high salt conditions, resulting in a significant decrease in the viscosity of the aqueous solution.
[0003] In recent years, with the continuous improvement of the degree of water injection development in my country's oil fields, the water content of the reservoir has also been increasing. It has been proposed to adjust the water absorption profile in the deep reservoir, force the flow to turn, and improve the recovery rate of water injection development. Gradually, a new hotspot in the research of deep adjustment and flooding technology has been formed, which plays an important role in stabilizing oil and controlling water. Accordingly, new chemical agents such as strong gel, weak gel, and granular gel have been developed. However, these chemical agents generally have poor fluidity, especially in the face of serious water flooding of oil wells in the ultra-high water content stage, complex oil-water relationship and other problems, and cannot achieve the purpose of deep adjustment and flooding of the reservoir. They can only work in the close area of the implementation well, resulting in a short on-site implementation period and poor results. Summary of the invention
[0004] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art and to provide an acrylamide copolymer and a preparation method and application thereof. The acrylamide copolymer has a higher viscosity under high temperature and high salt conditions, can enter deep into the oil reservoir, and can reduce the interfacial tension between the oil and water surfaces, and has better emulsification properties.
[0005] In order to achieve the above-mentioned object, the first aspect of the present invention provides an acrylamide copolymer, wherein the acrylamide copolymer comprises a structural unit A, a structural unit B and a structural unit C;
[0006] The structural unit A has a structure represented by formula (1), the structural unit B has a structure represented by formula (2), and the structural unit C has a structure represented by formula (3); based on the total weight of the acrylamide copolymer, the content of the structural unit A is 60-90% by weight, the content of the structural unit B is 5-35% by weight, and the content of the structural unit C is 1-8% by weight;
[0007]
[0008] Among them, R 1 , R 2 and R 3 Each independently is H or -CH 3 , M is Na or K.
[0009] A second aspect of the present invention provides a method for preparing an acrylamide copolymer, the method comprising:
[0010] 1) subjecting a monomer mixture to polymerization reaction in water under solution polymerization conditions and in the presence of an initiator to obtain a copolymer colloid; wherein the monomer mixture comprises (meth)acrylamide, a monomer X and a monomer Y, wherein the monomer X has a structure shown in formula (4), and the monomer Y has a structure shown in formula (5);
[0011] Based on the total amount of the monomer mixture, the amount of acrylamide is 60-90% by weight, the amount of the monomer X is 5-35% by weight, and the amount of the monomer Y is 1-8% by weight;
[0012]
[0013] 2) subjecting the copolymer colloid to a hydrolysis reaction to obtain an acrylamide copolymer;
[0014] Among them, R 2 ' and R 3 ' are each independently H or -CH 3 , M is Na or K.
[0015] The third aspect of the present invention provides an acrylamide copolymer prepared by the above method.
[0016] A fourth aspect of the present invention provides use of the acrylamide copolymer as a displacement agent in an oil field.
[0017] Through the above technical scheme, the acrylamide copolymer provided by the present invention and its preparation method and application can achieve the following beneficial effects:
[0018] The molecular chain of the acrylamide copolymer provided by the present invention contains a structural unit B from monomer X and a structural unit C from monomer Y, which greatly improves the temperature resistance and salt resistance of the copolymer and its surface and interfacial activity, and can effectively enter the deep part of the high-temperature and high-salt oil reservoir to achieve the purpose of deep flooding. The acrylamide copolymer can have a high viscosity under high temperature (100° C.) and high salinity (48000 mg / L) conditions, can enter the deep part of the oil reservoir, and can reduce the oil-water surface interfacial tension, and has good emulsification performance.
[0019] Further, in the present invention, in the preparation process of acrylamide copolymer, monomer Y containing superhydrophilic group and lipophilic group, monomer X containing sulfonic acid group and (methyl) acrylamide are polymerized, wherein monomer Y has good emulsification effect, and plays a self-emulsification role in the polymerization system, especially, under the action of promoter and urea, the polymerization activity of monomer is significantly improved, and the structural units of three copolymer monomers can be randomly distributed in the polymer chain, so that it has excellent viscosity and emulsification oil washing ability. Further, the sulfonic acid group contained in monomer X can greatly increase the temperature and salt resistance of the copolymer, and then effectively enhance the hydraulic volume between the molecular chains of the copolymer, so that the copolymer aqueous solution still maintains a very high viscosity under high temperature and high salt conditions, so as to achieve the purpose of deep flooding and plugging under the oil reservoir. DETAILED DESCRIPTION
[0020] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0021] The first aspect of the present invention provides an acrylamide copolymer, which comprises a structural unit A, a structural unit B and a structural unit C;
[0022] The structural unit A has a structure represented by formula (1), the structural unit B has a structure represented by formula (2), and the structural unit C has a structure represented by formula (3); based on the total weight of the acrylamide copolymer, the content of the structural unit A is 60-90% by weight, the content of the structural unit B is 5-35% by weight, and the content of the structural unit C is 1-8% by weight;
[0023]
[0024] Among them, R 1 , R 2 and R 3Each independently is H or -CH 3 , M is Na or K.
[0025] The inventors of the present invention have found in their research that by simultaneously introducing structural unit B and structural unit C into the macromolecular structure of polyacrylamide and controlling the content of each structural unit within the above range, the obtained acrylamide copolymer can have a higher viscosity under high temperature (100°C) and high mineralization (48000 mg / L) conditions, and can reduce the interfacial tension between the oil and water surfaces, has better emulsification properties, can adapt to the environment of severe oil well flooding and complex oil-water relationship, and achieve the purpose of deep profile control.
[0026] Furthermore, based on the total weight of the acrylamide copolymer, the content of the structural unit A is 75-82% by weight, the content of the structural unit B is 10-15% by weight, and the content of the structural unit C is 5-8% by weight.
[0027] In the present invention, the total content of the structural unit A, the structural unit B and the structural unit C is 100 wt %.
[0028] In the present invention, the content of each structural unit in the copolymer can be tested by conventional methods in the prior art, such as infrared spectroscopy, nuclear magnetic resonance, and the amount of monomers added during the polymerization process.
[0029] In the present invention, the content of each structural unit in the polymer is determined by the monomer feed amount. Specifically, the feed ratio of each monomer actually participating in the polymerization is determined by testing the content of unreacted monomers, and then the content of each structural unit in the polymer is determined.
[0030] Furthermore, in the present invention, when the content of each unreacted monomer in the tested polymer is less than 0.02 wt%, it indicates that substantially all monomers participate in the polymerization reaction. Specifically, the content of the residual monomer is determined by liquid chromatography.
[0031] In a preferred embodiment of the present invention, R 1 , R 3 and R 4 is H, M is Na.
[0032] In the present invention, under high temperature (greater than 100° C.) and high salt (mineralization degree of 48,000 mg / L) conditions, the apparent viscosity of the acrylamide copolymer aqueous solution is greater than 55 mPa·s, preferably greater than 63 mPa·s.
[0033] In the present invention, the apparent viscosity of the acrylamide copolymer aqueous solution is measured using a Brookfield viscometer. Specifically, the apparent viscosity of the acrylamide copolymer aqueous solution (mass concentration of 0.15 wt%) is measured at a specified test temperature (100° C.) and salinity (salinity of 48,000 mg / L).
[0034] A second aspect of the present invention provides a method for preparing an acrylamide copolymer, the method comprising:
[0035] 1) subjecting a monomer mixture to polymerization reaction in water under solution polymerization conditions and in the presence of an initiator to obtain a copolymer colloid; wherein the monomer mixture comprises (meth)acrylamide, a monomer X and a monomer Y, wherein the monomer X has a structure shown in formula (4), and the monomer Y has a structure shown in formula (5);
[0036] Based on the total amount of the monomer mixture, the amount of acrylamide is 60-90% by weight, the amount of the monomer X is 5-35% by weight, and the amount of the monomer Y is 1-8% by weight;
[0037]
[0038] 2) subjecting the copolymer colloid to a hydrolysis reaction to obtain an acrylamide copolymer;
[0039] Among them, R 2 ' and R 3 ' are each independently H or -CH 3 , M is Na or K.
[0040] In the present invention, (meth)acrylamide, the monomer X and the monomer Y are all commercially available.
[0041] In the present invention, the amount of the monomer mixture is 20-40 parts by weight relative to 100 parts by weight of water.
[0042] In the present invention, (methyl)acrylamide, a monomer X having a structure represented by formula (4) and a monomer Y having a structure represented by formula (5) are copolymerized to obtain an acrylamide copolymer. The copolymer has a high viscosity under high temperature (100° C.) and high mineralization (48000 mg / L) conditions, can penetrate deep into the oil reservoir, can reduce the interfacial tension between the oil and water surfaces, and has good emulsification properties.
[0043] Furthermore, based on the total weight of the monomer mixture, the amount of the (meth)acrylamide is 75-82% by weight, the amount of the monomer X is 10-15% by weight, and the amount of the monomer Y is 5-8% by weight.
[0044] According to the present invention, the conditions of the solution polymerization reaction include: the initiator is an oxidation-reduction system initiator; the reaction temperature is 30-60° C., the reaction time is 6-8 hours, and the pH value is 6-8.
[0045] In the present invention, the conventional means in the prior art can be used, for example, by adding alkaline substances such as sodium hydroxide to adjust the pH value of the polymerization reaction system.
[0046] According to the present invention, the conditions for the solution polymerization reaction also include: being carried out under an inert atmosphere.
[0047] In the present invention, a conventional atmosphere capable of providing an inert environment in the art, such as nitrogen, may be used.
[0048] According to the present invention, the amount of the initiator is 0.015-0.15 parts by weight relative to 100 parts by weight of the monomer mixture.
[0049] In the present invention, the oxidation-reduction system initiator can be a conventional oxidation-reduction system initiator in the art, preferably a persulfate oxidant and a sulfite reducer.
[0050] Specifically, the persulfate oxidant may be, for example, potassium persulfate, ammonium persulfate, etc. The sulfite may be, for example, potassium bisulfite, sodium bisulfite, etc. Preferably, relative to 100 parts by weight of the monomer mixture, the persulfate oxidant is 0.01-0.1 parts by weight; the sulfite reducing agent is 0.005-0.05 parts by weight.
[0051] According to the present invention, the conditions of the solution polymerization reaction also include: being carried out in the presence of a complexing agent, urea and a promoter.
[0052] In the present invention, the influence of impurities on polymerization activity can be significantly reduced through the complexing effect of the complexing agent, while the addition of urea significantly increases the water solubility of the copolymer, and the introduction of the accelerator can further improve the viscosity and emulsification properties of the prepared acrylamide copolymer.
[0053] According to the present invention, relative to 100 parts by weight of the monomer mixture, the complexing agent is 0.01-0.1 parts by weight, the urea is 0.5-5 parts by weight, and the accelerator is 0.05-0.5 parts by weight.
[0054] According to the present invention, the complexing agent is disodium ethylenediaminetetraacetate (EDTA-2Na), and the accelerator is 1,3-bis(4-methoxyphenyl)thiourea.
[0055] In the present invention, the hydrolysis reaction can be carried out under alkaline conditions, and the alkaline conditions can be achieved by adding sodium hydroxide granules and other substances. There is no particular limitation on the amount of alkaline substance added, and those skilled in the art can adjust it according to the needs of the reaction. Preferably, the conditions of the hydrolysis reaction include: a temperature of 80-90° C. and a time of 2-3 h.
[0056] In the present invention, preferably, after the hydrolysis reaction, the reaction product is granulated, dried, crushed and sieved to obtain the acrylamide copolymer.
[0057] In a preferred embodiment of the present invention, the method for preparing the acrylamide copolymer comprises:
[0058] 1) preparing (meth)acrylamide into an aqueous solution, then adding monomer X, monomer Y, complex aqueous solution, urea and accelerator, adjusting the pH value, and stirring sufficiently to make it a stable solution;
[0059] 2) adding an oxidation-reduction system initiator, blowing in an inert gas to mix evenly, sealing and polymerizing to obtain a polymer colloid;
[0060] 3) Taking out the colloid, adding alkaline substances after granulation, mixing it evenly and then carrying out hydrolysis reaction;
[0061] 4) Granulating, drying, crushing and screening the hydrolysis reaction product to obtain an acrylamide copolymer.
[0062] The third aspect of the present invention provides an acrylamide copolymer prepared by the above method.
[0063] A fourth aspect of the present invention provides use of the acrylamide copolymer as a displacement agent in an oil field.
[0064] The acrylamide copolymer provided by the present invention has high viscosity under high temperature (100°C) and high mineralization (48000mg / L) conditions, can enter deep oil reservoirs, and can reduce oil-water surface interfacial tension, has good emulsification properties, and can be applied to profile control agents to achieve deep profile control.
[0065] The present invention will be described in detail below by way of examples. In the following examples,
[0066] Unless otherwise specified, all raw materials are commercially available. 2 ' is H, M is Na; in X2, R 2 ' is H, M is K) was purchased from Dongying Baomo Environmental Engineering Co., Ltd., and the monomer Y (in Y1, R 3 ' is H; in Y2, R 3 'For CH 3) was purchased from Bailingwei Technology Co., Ltd.
[0067] Example 1
[0068] 1) Add 270g of acrylamide to a heat-insulating polymerization reaction bottle, add 900g of deionized water to dissolve and prepare an aqueous solution, add 27g of monomer X1, 3g of monomer Y1, 0.1g of EDTA-2Na, 1.5g of urea, 0.15g of 1,3-bis(4-methoxyphenyl)thiourea in sequence, add sodium hydroxide to adjust the pH to 7, and stir thoroughly to form a stable solution;
[0069] 2) At 20° C., nitrogen was passed through the solution to drive out oxygen for 30 minutes, and then 5 g of a 1 wt % aqueous solution of potassium persulfate and 2.5 g of a 1 wt % aqueous solution of sodium bisulfite were added to initiate the reaction. The nitrogen was continued to be passed through for five minutes and then stopped. After sealing, the solution was polymerized for 8 hours to obtain a polymer colloid;
[0070] 3) Take out the colloid, granulate it, add 33.8g of sodium hydroxide granules, mix well, and perform hydrolysis reaction at 90°C for 2 hours;
[0071] 4) The granules were taken out and granulated, dried at 60° C. to constant weight, crushed, and sieved to obtain white granular acrylamide copolymer J1.
[0072] According to the calculation determined by the feed amount, based on the total weight of the acrylamide copolymer J1, the content of the structural unit A is 90 weight %, the content of the structural unit B is 9 weight % and the content of the structural unit C is 1 weight %.
[0073] Example 2
[0074] 1) Add 180g acrylamide to a heat-insulating polymerization reaction bottle, add 900g deionized water to dissolve and prepare an aqueous solution, add 1105g monomer X1, 15g monomer Y1, 0.03g EDTA-2Na, 6g urea, 0.3g 1,3-bis(4-methoxyphenyl)thiourea in sequence, add sodium hydroxide to adjust the pH to 8, and stir thoroughly to form a stable solution;
[0075] 2) At 10° C., nitrogen was passed through the solution to drive out oxygen for 30 minutes, and then 10 g of a 1 wt % aqueous solution of potassium persulfate and 5 g of a 1 wt % aqueous solution of sodium bisulfite were added to initiate the reaction. The nitrogen was continued to be passed through for five minutes and then stopped. After sealing, the solution was polymerized for 10 hours to obtain a polymer colloid;
[0076] 3) Take out the colloid, granulate it, add 30.4g of sodium hydroxide granules, mix well, and perform hydrolysis reaction at 90°C for 2 hours;
[0077] 4) The granules were taken out and granulated, dried at 60° C. to constant weight, crushed, and sieved to obtain white granular acrylamide copolymer J2.
[0078] According to the calculation determined by the feed amount, based on the total weight of the acrylamide copolymer J2, the content of the structural unit A is 60 weight %, the content of the structural unit B is 35 weight % and the content of the structural unit C is 5 weight %.
[0079] Example 3
[0080] 1) Add 240g acrylamide to a heat-insulating polymerization reaction bottle, add 900g deionized water to dissolve and prepare an aqueous solution, add 136g monomer X, 124g monomer Y, 0.3g EDTA-2Na, 15g urea, 1.5g 1,3-bis(4-methoxyphenyl)thiourea in sequence, add sodium hydroxide to adjust the pH to 6, and stir thoroughly to form a stable solution;
[0081] 2) At 15° C., nitrogen was passed through the solution to drive out oxygen for 30 minutes, and then 30 g of a 1 wt % aqueous solution of potassium persulfate and 15 g of a 1 wt % aqueous solution of sodium bisulfite were added to initiate the reaction. The nitrogen was continued to be passed through for five minutes and then stopped. After sealing, the solution was polymerized for 8 hours to obtain a polymer colloid;
[0082] 3) Take out the colloid, granulate it, add 37.2g of sodium hydroxide granules, mix well, and perform hydrolysis reaction at 90°C for 2 hours;
[0083] 4) The granules were taken out and granulated, dried at 60° C. to constant weight, crushed, and sieved to obtain white granular acrylamide copolymer J3.
[0084] According to the calculation determined by the feed amount, based on the total weight of the acrylamide copolymer J3, the content of the structural unit A is 80 weight %, the content of the structural unit B is 12 weight % and the content of the structural unit C is 8 weight %.
[0085] Example 4
[0086] 1) Add 264 g of acrylamide to a heat-insulating polymerization reaction bottle, add 900 g of deionized water to dissolve and prepare an aqueous solution, add 115 g of monomer X, 121 g of monomer Y, 0.2 g of EDTA-2Na, 12 g of urea, 1.1 g of 1,3-bis(4-methoxyphenyl)thiourea in sequence, add sodium hydroxide to adjust the pH to 7, and stir thoroughly to form a stable solution;
[0087] 2) At 10° C., nitrogen was passed through the solution to drive out oxygen for 30 minutes, and then 15 g of a 1 wt % aqueous solution of potassium persulfate and 7.5 g of a 1 wt % aqueous solution of sodium bisulfite were added to initiate the reaction. The nitrogen was continued to be passed through for five minutes and then stopped. After sealing, the solution was polymerized for 10 hours to obtain a polymer colloid;
[0088] 3) Take out the colloid, granulate it, add 32.1g of sodium hydroxide granules, mix well, and then carry out hydrolysis reaction at 90°C for 2 hours;
[0089] 4) The granules were taken out and granulated, dried at 60° C. to constant weight, crushed, and sieved to obtain white granular acrylamide copolymer J4.
[0090] According to the calculation based on the feed amount, based on the total weight of the acrylamide copolymer J4, the content of the structural unit A is 88% by weight, the content of the structural unit B is 5% by weight, and the content of the structural unit C is 7% by weight.
[0091] Example 5
[0092] An acrylamide copolymer was prepared according to the method of Example 1, except that methacrylamide was used instead of acrylamide to obtain an acrylamide copolymer J5.
[0093] According to the calculation determined by the feed amount, based on the total weight of the acrylamide copolymer J5, the content of the structural unit A is 90 weight %, the content of the structural unit B is 9 weight % and the content of the structural unit C is 1 weight %.
[0094] Example 6
[0095] An acrylamide copolymer was prepared according to the method of Example 1, except that monomer X2 was used instead of monomer X1 to obtain acrylamide copolymer J6.
[0096] According to the calculation determined by the feed amount, based on the total weight of the acrylamide copolymer J6, the content of the structural unit A is 90 weight %, the content of the structural unit B is 9 weight % and the content of the structural unit C is 1 weight %.
[0097] Example 7
[0098] An acrylamide copolymer was prepared according to the method of Example 1, except that monomer Y2 was used to replace monomer Y1, to obtain acrylamide copolymer J7.
[0099] According to the calculation determined by the feed amount, based on the total weight of the acrylamide copolymer J7, the content of the structural unit A is 90 weight %, the content of the structural unit B is 9 weight % and the content of the structural unit C is 1 weight %.
[0100] Comparative Example 1
[0101] An acrylamide copolymer was prepared according to the method of Example 1, except that an equal mass of monomer X was used instead of monomer Y to obtain an acrylamide copolymer D1.
[0102] According to the calculation determined by the feed amount, based on the total weight of the acrylamide copolymer D1, the content of the structural unit A is 90 weight %, the content of the structural unit B is 10 weight % and the content of the structural unit C is 0 weight %.
[0103] Comparative Example 2
[0104] An acrylamide copolymer was prepared according to the method of Example 1, except that an equal mass of monomer Y was used instead of monomer X to obtain an acrylamide copolymer D2.
[0105] According to the calculation determined by the feed amount, based on the total weight of the acrylamide copolymer D2, the content of the structural unit A is 90 weight %, the content of the structural unit B is 0 weight % and the content of the structural unit C is 10 weight %.
[0106] Comparative Example 3
[0107] An acrylamide copolymer was prepared according to the method of Example 1, except that the amount of acrylamide used was 150 g, the amount of monomer X used was 120 g, and the amount of monomer Y used was 30 g. Acrylamide copolymer D3 was obtained.
[0108] According to the calculation determined by the feed amount, based on the total weight of the acrylamide copolymer D3, the content of the structural unit A is 50 weight %, the content of the structural unit B is 40 weight % and the content of the structural unit C is 10 weight %.
[0109] Test Case
[0110] The acrylamide copolymers obtained in the examples and comparative examples were respectively prepared into 0.15 wt % aqueous solutions, and the apparent viscosity, surface tension and interfacial tension of each aqueous solution were measured. The test results are shown in Table 1.
[0111] The apparent viscosity of the acrylamide copolymer aqueous solution was measured by a Brookfield viscometer, the test temperature was 100°C, and the mineralization was 48000 mg / L;
[0112] The surface tension of the acrylamide copolymer aqueous solution in pure water was measured by a DCAT-21 surface tension meter at a test temperature of 25°C;
[0113] The interfacial tension of the acrylamide copolymer aqueous solution was measured by a TX500C interfacial tension meter from the American Kono Company. The test temperature was 100°C and the experimental oil was crude oil from Shengli Oilfield.
[0114] Table 1
[0115]
[0116]
[0117] It can be seen from the results in Table 1 that the acrylamide copolymer provided by the present invention has a higher apparent viscosity under the conditions of a temperature of 100° C. and a mineralization of 48000 mg / L, showing excellent high temperature and high salt resistance; at the same time, it has lower surface tension and interfacial tension, showing excellent surface activity.
[0118] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing an acrylamide copolymer, It is characterized in that The method comprises: 1) subjecting a monomer mixture to a solution polymerization reaction in water under solution polymerization conditions and in the presence of an initiator to obtain a copolymer colloid; wherein the monomer mixture comprises (meth)acrylamide, a monomer X and a monomer Y, wherein the monomer X has a structure shown in formula (4), and the monomer Y has a structure shown in formula (5); Based on the total amount of the monomer mixture, the amount of (meth)acrylamide is 60-90% by weight, the amount of the monomer X is 5-35% by weight, and the amount of the monomer Y is 1-8% by weight; 2) subjecting the copolymer colloid to a hydrolysis reaction to obtain an acrylamide copolymer; Among them, R 2 ' and R 3 ' are each independently H or -CH 3 , M is Na or K.
2. The method according to claim 1, in, The conditions of the solution polymerization reaction include: the initiator is an oxidation-reduction system initiator; the reaction temperature is 30-60° C., the reaction time is 6-8 hours, and the pH value is 6-8.
3. The method according to claim 1, in, The conditions of the solution polymerization reaction also include: being carried out under an inert atmosphere.
4. The method according to claim 1, in, The amount of the initiator used is 0.015-0.15 parts by weight relative to 100 parts by weight of the monomer mixture.
5. The method according to claim 2, in, The oxidation-reduction system initiator is a persulfate oxidant and a sulfite reducer.
6. The method according to claim 5, in, Relative to 100 parts by weight of the monomer mixture, the persulfate oxidizing agent is 0.01-0.1 parts by weight; and the sulfite reducing agent is 0.005-0.05 parts by weight.
7. The method according to any one of claims 1 to 6, in, The conditions of the solution polymerization reaction also include: being carried out in the presence of a complexing agent, urea and a promoter.
8. The method according to claim 7, in, Relative to 100 parts by weight of the monomer mixture, the complexing agent is 0.01-0.1 parts by weight, the urea is 0.5-5 parts by weight, and the accelerator is 0.05-0.5 parts by weight.
9. The method according to claim 7, in, The complexing agent is disodium ethylenediaminetetraacetate, and the accelerator is 1,3-bis(4-methoxyphenyl)thiourea.
10. Acrylamide copolymer obtained by the method according to any one of claims 1 to 9.
11. Use of the acrylamide copolymer according to claim 10 as a displacement agent in an oil field.
Citation Information
Patent Citations
Acrylamide copolymer as well as preparation method and application thereof
CN109232805A
Acrylamide copolymer as well as preparation method and application thereof
CN109232810A
Oil recovery chemical and method for producing the same, and injection liquid for recovering oil
JP2010270170A