Acrylamide polymer and its preparation method and application

By introducing specific structural units and groups into the polymer, the temperature resistance and salt resistance and emulsification properties of acrylamide polymers are improved, and the problem of the polymer's viscosity decrease under high temperature and high salt conditions is solved, and the effective reservoir depth is achieved Adjust the drive and blockage.

CN115677919BActive Publication Date: 2024-11-19CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110859279.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-28
Publication Date
2024-11-19
Estimated Expiration
2041-07-28

AI Technical Summary

Technical Problem

The viscosity of existing polymers decreases under high temperature and high salt conditions, and cannot effectively enter the deep reservoir, resulting in poor oil displacement effect, especially in deep-dumping and blocking.

Method used

Using acrylamide polymer, the temperature resistance and salt resistance of the polymer are improved and the surface interface activity are combined with superhydrophilic groups and lipophilic groups by introducing structural units B and structural units C into the polymer and controlling their content. The monomer undergoes polymerization reaction to enhance the emulsification properties and viscosity of the polymer.

Benefits of technology

Under high temperature and high salt conditions, acrylamide polymer can maintain high viscosity, enter the deep oil reservoir, reduce the interface tension of the oil and water meter, achieve the purpose of deep driving and blockage, and adapt to environments with severe flooding of oil wells and complex oil-water relationships.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115677919B_ABST
    Figure CN115677919B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of oilfield chemicals, and discloses an acrylamide polymer and a preparation method and application thereof. The acrylamide polymer comprises a structural unit A, a structural unit B and a structural unit C; the structural unit A has a structure shown in formula (1), the structural unit B has a structure shown in formula (2), and the structural unit C has a structure shown in formula (3); based on the total weight of the acrylamide polymer, the content of the structural unit A is 80-90% by weight, the content of the structural unit B is 5-15% by weight, and the content of the structural unit C is 1-5% by weight; #imgabs0# wherein, R 1 , R 2 and R 3 Each is independently H or -CH 3 , R 4 The acrylamide polymer has a high viscosity under high temperature and high salt conditions, can enter deep into the oil reservoir, and can reduce the interfacial tension between the oil and water surfaces, and has good emulsification properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of oilfield chemicals, and in particular to an acrylamide polymer and a preparation method and application thereof. Background Art

[0002] In tertiary oil recovery, the use of water-soluble polymer flooding has developed into an extremely important technology for improving oil recovery. Water-soluble polymers have good water solubility and viscosity-increasing properties. When they are added to water, the viscosity of the aqueous solution can be significantly increased, the water / oil mobility ratio under the reservoir can be reduced, and the fluid swept volume and sweep efficiency can be increased, and the oil saturation in the swept area can be reduced, thereby achieving the purpose of improving oil recovery. The results of the field implementation in the oil field show that the use of polymer flooding can greatly improve the recovery of crude oil and generate huge economic and social benefits. At present, due to the curling and rapid degradation of polymer molecular chains under high temperature and high salt conditions, the viscosity of the aqueous solution is greatly reduced, which in turn significantly reduces the oil recovery effect of the polymer under high temperature and high salt conditions.

[0003] In recent years, with the continuous improvement of the degree of water injection development in my country's oil fields, the water content of the reservoir has also been increasing. It has been proposed to adjust the water absorption profile in the deep reservoir, force the flow to turn, and improve the recovery rate of water injection development. Gradually, a new hotspot in the research of deep adjustment and flooding technology has been formed, which plays an important role in stabilizing oil and controlling water. Accordingly, new chemical agents such as strong gel, weak gel, and granular gel have been developed. However, these chemical agents generally have poor fluidity, especially in the face of serious water flooding of oil wells in the ultra-high water content stage, complex oil-water relationship and other problems, and cannot achieve the purpose of deep adjustment and flooding of the reservoir. They can only work in the close area of ​​the implementation well, resulting in a short on-site implementation period and poor results. Summary of the invention

[0004] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art and to provide an acrylamide polymer and a preparation method and application thereof. The acrylamide polymer has a higher viscosity under high temperature and high salt conditions, can enter deep into the oil reservoir, and can reduce the interfacial tension between the oil and water surfaces and has better emulsification properties.

[0005] In order to achieve the above object, the first aspect of the present invention provides an acrylamide polymer, which comprises a structural unit A, a structural unit B and a structural unit C;

[0006] The structural unit A has a structure shown in formula (1), the structural unit B has a structure shown in formula (2), and the structural unit C has a structure shown in formula (3); based on the total weight of the acrylamide polymer, the content of the structural unit A is 80-90% by weight, the content of the structural unit B is 5-15% by weight, and the content of the structural unit C is 1-5% by weight;

[0007]

[0008] Wherein, R1, R2 and R3 are each independently H or -CH3, and R4 is methyl or ethyl.

[0009] A second aspect of the present invention provides a method for preparing an acrylamide polymer, the method comprising:

[0010] (1) subjecting a monomer mixture to a polymerization reaction in water under solution polymerization conditions and in the presence of an initiator to obtain a polymer colloid; wherein the monomer mixture comprises (meth)acrylamide, a monomer X and a monomer Y, wherein the monomer X has a structure represented by formula (4), and the monomer Y has a structure represented by formula (5);

[0011] Based on the total amount of the monomer mixture, the amount of acrylamide is 80-90% by weight, the amount of the monomer X is 5-15% by weight, and the amount of the monomer Y is 1-5% by weight;

[0012]

[0013] (2) subjecting the polymer colloid to a hydrolysis reaction to obtain an acrylamide polymer;

[0014] Wherein, R2' and R3' are each independently H or -CH3, and R4' is methyl or ethyl.

[0015] The third aspect of the present invention provides an acrylamide polymer prepared by the above method.

[0016] A fourth aspect of the present invention provides use of the acrylamide polymer as a displacement agent in an oil field.

[0017] Through the above technical scheme, the acrylamide polymer provided by the present invention and its preparation method and application obtain the following beneficial effects:

[0018] The molecular chain of the acrylamide polymer provided by the present invention contains the structural unit B from the monomer X and the structural unit C from the monomer Y, which greatly improves the temperature resistance and salt resistance and the surface and interfacial activity of the polymer, and can effectively enter the deep part of the high-temperature and high-salt oil reservoir to achieve the purpose of deep flooding. The acrylamide polymer can have a high viscosity under the conditions of high temperature (100° C.) and high salinity (48000 mg / L), can enter the deep part of the oil reservoir, and can reduce the oil-water surface interfacial tension, and has good emulsification performance.

[0019] Further, in the present invention, in the preparation process of acrylamide polymer, monomer Y containing superhydrophilic group and lipophilic group, nonionic functional monomer X containing large side group and (methyl) acrylamide are polymerized, wherein monomer Y has good emulsification effect, plays a self-emulsification role in the polymerization system, and in particular, under the action of promoter and urea, the polymerization activity of monomer is significantly improved, and the structural units of three polymerization monomers can be randomly distributed in the polymer chain, thereby making it have excellent viscosity and emulsification oil washing ability. Further, the large side group contained in the nonionic functional monomer X can reduce the influence of salt ions, enhance the temperature resistance and salt resistance of the polymer, and then effectively enhance the hydraulic volume between polymer molecular chains, so that the polymer aqueous solution still maintains a high viscosity under high temperature and high salt conditions, thereby achieving the purpose of deep flooding and plugging under the oil reservoir. DETAILED DESCRIPTION

[0020] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0021] The first aspect of the present invention provides an acrylamide polymer, wherein the acrylamide polymer comprises a structural unit A, a structural unit B and a structural unit C;

[0022] The structural unit A has a structure shown in formula (1), the structural unit B has a structure shown in formula (2), and the structural unit C has a structure shown in formula (3); based on the total weight of the acrylamide polymer, the content of the structural unit A is 80-90% by weight, the content of the structural unit B is 5-15% by weight, and the content of the structural unit C is 1-5% by weight;

[0023]

[0024] Wherein, R1, R2 and R3 are each independently H or -CH3, and R4 is methyl or ethyl.

[0025] The inventors of the present invention have found in their research that by simultaneously introducing structural unit B and structural unit C into the macromolecular structure of polyacrylamide and controlling the content of each structural unit within the above range, the obtained acrylamide polymer has a higher viscosity under high temperature (100°C) and high mineralization (48000 mg / L) conditions, can reduce the interfacial tension between the oil and water surfaces, has good emulsification properties, can adapt to the environment of severe oil well flooding and complex oil-water relationship, and achieve the purpose of deep profile control.

[0026] Furthermore, based on the total weight of the acrylamide polymer, the content of the structural unit A is 80-85% by weight, the content of the structural unit B is 10-15% by weight, and the content of the structural unit C is 3-5% by weight.

[0027] In the present invention, the total content of the structural unit A, the structural unit B and the structural unit C is 100 wt %.

[0028] In the present invention, the content of each structural unit in the polymer can be tested by conventional methods in the prior art, such as infrared spectroscopy, nuclear magnetic resonance, and the amount of monomers added during the polymerization process.

[0029] In the present invention, the content of each structural unit in the polymer is determined by the monomer feed amount. Specifically, the feed ratio of each monomer actually participating in the polymerization is determined by testing the content of unreacted monomers, and then the content of each structural unit in the polymer is determined.

[0030] Furthermore, in the present invention, when the content of each unreacted monomer in the tested polymer is less than 0.02 wt%, it indicates that substantially all monomers participate in the polymerization reaction. Specifically, the content of the residual monomer is determined by liquid chromatography.

[0031] In a preferred embodiment of the present invention, R1, R2 and R3 are H, and R4 is ethyl.

[0032] In the present invention, under high temperature (greater than 100° C.) and high salt (mineralization degree of 48,000 mg / L) conditions, the apparent viscosity of the acrylamide polymer aqueous solution is greater than 58 mPa·s, preferably greater than 65 mPa·s.

[0033] In the present invention, the apparent viscosity of the acrylamide polymer aqueous solution is measured using a Brookfield viscometer. Specifically, the apparent viscosity of the acrylamide polymer aqueous solution (mass concentration of 0.15 wt%) is measured at a specified test temperature (100° C.) and salinity (salinity of 48,000 mg / L).

[0034] A second aspect of the present invention provides a method for preparing an acrylamide polymer, characterized in that the method comprises:

[0035] (1) subjecting a monomer mixture to a polymerization reaction in water under solution polymerization conditions and in the presence of an initiator to obtain a polymer colloid; wherein the monomer mixture comprises (meth)acrylamide, a monomer X and a monomer Y, wherein the monomer X has a structure represented by formula (4), and the monomer Y has a structure represented by formula (5);

[0036] Based on the total amount of the monomer mixture, the amount of acrylamide is 80-90% by weight, the amount of the monomer X is 5-15% by weight, and the amount of the monomer Y is 1-5% by weight;

[0037]

[0038] (2) subjecting the polymer colloid to a hydrolysis reaction to obtain an acrylamide polymer;

[0039] Wherein, R2' and R3' are each independently H or -CH3, and R4' is methyl or ethyl.

[0040] In the present invention, (meth)acrylamide, the monomer X and the monomer Y are all commercially available.

[0041] In the present invention, the amount of the monomer mixture is 20-40 parts by weight relative to 100 parts by weight of water.

[0042] In the present invention, (methyl)acrylamide, a monomer X having a structure represented by formula (4) and a monomer Y having a structure represented by formula (5) are copolymerized to obtain an acrylamide polymer. The polymer has a high viscosity under high temperature (100° C.) and high mineralization (48000 mg / L) conditions, can penetrate deep into the oil reservoir, can reduce the interfacial tension between the oil and water surfaces, and has good emulsification properties.

[0043] In a preferred embodiment of the present invention, R2' and R3' are H, and R4' is ethyl.

[0044] Furthermore, based on the total weight of the monomer mixture, the amount of the (meth)acrylamide is 80-85% by weight, the amount of the monomer X is 10-15% by weight, and the amount of the monomer Y is 3-5% by weight.

[0045] According to the present invention, the conditions of the solution polymerization reaction include: the initiator is an oxidation-reduction system initiator; the reaction temperature is 10-20° C., the reaction time is 8-10 h, and the pH value is 6-8.

[0046] In the present invention, the conventional means in the prior art can be used, for example, by adding alkaline substances such as sodium hydroxide to adjust the pH value of the polymerization reaction system.

[0047] According to the present invention, the conditions for the solution polymerization reaction also include: being carried out under an inert atmosphere.

[0048] In the present invention, a conventional atmosphere capable of providing an inert environment in the art, such as nitrogen, may be used.

[0049] According to the present invention, the amount of the initiator is 0.015-0.15 parts by weight relative to 100 parts by weight of the monomer mixture.

[0050] According to the present invention, the oxidation-reduction system initiator is a persulfate oxidant and a sulfite reductant.

[0051] In the present invention, the oxidation-reduction system initiator can be a conventional oxidation-reduction system initiator in the art, preferably a persulfate oxidant and a sulfite reducer.

[0052] Specifically, the persulfate oxidant may be, for example, potassium persulfate, ammonium persulfate, etc. The sulfite may be, for example, potassium bisulfite, sodium bisulfite, etc. Preferably, relative to 100 parts by weight of the monomer mixture, the persulfate oxidant is 0.01-0.1 parts by weight; the sulfite reducing agent is 0.005-0.05 parts by weight.

[0053] According to the present invention, the conditions of the solution polymerization reaction also include: being carried out in the presence of a complexing agent, urea and a promoter.

[0054] In the present invention, the influence of impurities on polymerization activity can be significantly reduced through the complexing effect of the complexing agent, the introduction of urea can significantly increase the water solubility of the copolymer, and the introduction of the accelerator can further improve the viscosity and emulsification properties of the prepared acrylamide polymer.

[0055] According to the present invention, relative to 100 parts by weight of the monomer mixture, the complexing agent is 0.01-0.1 parts by weight, the urea is 0.5-5 parts by weight, and the accelerator is 0.05-0.5 parts by weight.

[0056] According to the present invention, the complexing agent is disodium ethylenediaminetetraacetate (EDTA-2Na), and the accelerator is 1,3-bis(4-methoxyphenyl)thiourea.

[0057] In the present invention, the hydrolysis reaction can be carried out under alkaline conditions, and the alkaline conditions can be achieved by adding sodium hydroxide granules and other substances. There is no particular limitation on the amount of alkaline substance added, and those skilled in the art can adjust it according to the needs of the reaction. Preferably, the conditions of the hydrolysis reaction include: a temperature of 80-90°C and a time of 2-3h.

[0058] Preferably, after the hydrolysis reaction, the reaction product is granulated, dried, crushed and sieved to obtain the acrylamide polymer.

[0059] In a preferred embodiment of the present invention, the method for preparing acrylamide polymer comprises:

[0060] 1) adding (meth)acrylamide into a reactor to prepare an aqueous solution, then adding monomer X, monomer Y, complex aqueous solution, urea and accelerator, adjusting the pH value, and stirring sufficiently to make it a stable solution;

[0061] 2) adding an oxidation-reduction system initiator, blowing in an inert gas to mix evenly, sealing and polymerizing to obtain a polymer colloid;

[0062] 3) Taking out the colloid, adding alkaline substances after granulation, mixing it evenly and then carrying out hydrolysis reaction;

[0063] 4) Granulating, drying, crushing and screening the hydrolysis reaction product to obtain an acrylamide polymer.

[0064] The third aspect of the present invention provides an acrylamide polymer prepared by the above method.

[0065] The acrylamide polymer provided by the present invention has high viscosity under high temperature (100°C) and high mineralization (48000mg / L) conditions, can enter deep oil reservoirs, and can reduce oil-water surface interfacial tension, has good emulsification properties, and can be applied to profile control agents to achieve deep profile control.

[0066] A fourth aspect of the present invention provides use of the acrylamide polymer as a displacement agent in an oil field.

[0067] The present invention will be described in detail below by way of examples. In the following examples,

[0068] Unless otherwise specified, all raw materials were purchased from commercial sources. Among them, the monomer X represented by formula (4) (in X1, R2' is H; in X2, R2' is CH3) was purchased from Bailingwei Technology Co., Ltd., and the monomer Y represented by formula (5) (in Y1, R3' is H, R4' is ethyl; in Y2, R3' is H, R4' is methyl) was purchased from Beijing Inokai Technology Co., Ltd.

[0069] Example 1

[0070] 1) Add 240g acrylamide to a heat-insulating polymerization reaction bottle, add 900g deionized water to dissolve and prepare an aqueous solution, add 145g monomer X, 15g monomer Y1, 0.2g EDTA-2Na, 15g urea, 1.5g 1,3-bis(4-methoxyphenyl)thiourea in sequence, add sodium hydroxide to adjust the pH to 8, and stir thoroughly to form a stable solution;

[0071] 2) At 20° C., nitrogen was passed through the solution to drive out oxygen for 30 minutes, and then 20 g of a 1 wt % aqueous solution of potassium persulfate and 10 g of a 1 wt % aqueous solution of sodium bisulfite were added to initiate the reaction, and nitrogen was continued to be passed through for five minutes before stopping. After sealing, the solution was polymerized for 10 hours to obtain a polymer colloid;

[0072] 3) Take out the colloid, granulate it, add 37.2g of sodium hydroxide granules, mix well, and perform hydrolysis reaction at 80°C for 3 hours;

[0073] 4) The granules were taken out and granulated, dried at 60° C. to constant weight, crushed, and sieved to obtain white granular acrylamide polymer J1.

[0074] According to the calculation determined by the feed amount, based on the total weight of the acrylamide polymer J1, the content of the structural unit A is 80 weight %, the content of the structural unit B is 15 weight % and the content of the structural unit C is 5 weight %.

[0075] Example 2

[0076] 1) Add 264 g of acrylamide to a heat-insulating polymerization reaction bottle, add 900 g of deionized water to dissolve and prepare an aqueous solution, add 30 g of monomer X1, 16 g of monomer Y, 0.1 g of EDTA-2Na, 8 g of urea, and 0.5 g of 1,3-bis(4-methoxyphenyl)thiourea in sequence, then add sodium hydroxide to adjust the pH to 6, and stir thoroughly to form a stable solution;

[0077] 2) At 10° C., nitrogen was passed through the solution to drive out oxygen for 30 minutes, and then 15 g of a 1 wt % aqueous solution of potassium persulfate and 7.5 g of a 1 wt % aqueous solution of sodium bisulfite were added to initiate the reaction. The nitrogen was continued to be passed through for five minutes and then stopped. After sealing, the solution was polymerized for 8 hours to obtain a polymer colloid;

[0078] 3) Take out the colloid, granulate it, add 33.8g of sodium hydroxide granules, mix well, and perform hydrolysis reaction at 85°C for 2 hours;

[0079] 4) The granules were taken out and granulated, dried at 60° C. to constant weight, crushed, and sieved to obtain white granular acrylamide polymer J2.

[0080] According to the calculation determined by the feed amount, based on the total weight of the acrylamide polymer J2, the content of the structural unit A is 88% by weight, the content of the structural unit B is 10% by weight, and the content of the structural unit C is 2% by weight.

[0081] Example 3

[0082] 1) Add 270g of acrylamide to a heat-insulating polymerization reaction bottle, add 900g of deionized water to dissolve and prepare an aqueous solution, add 127g of monomer X, 13g of monomer Y, 0.03g of EDTA-2Na, 5g of urea, 0.15g of 1,3-bis(4-methoxyphenyl)thiourea in sequence, add sodium hydroxide to adjust the pH to 7, and stir thoroughly to form a stable solution;

[0083] 2) At 15° C., nitrogen was passed through the solution to drive out oxygen for 30 minutes, and then 8 g of a 1 wt % aqueous solution of potassium persulfate and 4 g of a 1 wt % aqueous solution of sodium bisulfite were added to initiate the reaction. The nitrogen was continued to be passed through for five minutes and then stopped. After sealing, the solution was polymerized for 7 hours to obtain a polymer colloid;

[0084] 3) Take out the colloid, granulate it, add 32.1g of sodium hydroxide granules, mix well, and then carry out hydrolysis reaction at 90°C for 2 hours;

[0085] 4) The granules were taken out and granulated, dried at 60° C. to constant weight, crushed, and sieved to obtain white granular acrylamide polymer J3.

[0086] According to the calculation determined by the feed amount, based on the total weight of the acrylamide polymer J3, the content of the structural unit A is 90 weight %, the content of the structural unit B is 9 weight % and the content of the structural unit C is 1 weight %.

[0087] Example 4

[0088] 1) Add 270g of acrylamide to a heat-insulating polymerization reaction bottle, add 900g of deionized water to dissolve and prepare an aqueous solution, add 115g of monomer X, 115g of monomer Y, 0.3g of EDTA-2Na, 10g of urea, 1.0g of 1,3-bis(4-methoxyphenyl)thiourea in sequence, add sodium hydroxide to adjust the pH to 7.2, and stir thoroughly to form a stable solution;

[0089] 2) At 17.5° C., nitrogen was passed through the solution to drive out oxygen for 30 minutes, and then 30 g of a 1 wt % aqueous solution of potassium persulfate and 15 g of a 1 wt % aqueous solution of sodium bisulfite were added to initiate the reaction, and nitrogen was continued to be passed through for five minutes before stopping. After sealing, the solution was polymerized for 10 hours to obtain a polymer colloid;

[0090] 3) Take out the colloid, granulate it, add 35.5g of sodium hydroxide granules, mix well, and then carry out hydrolysis reaction at 85°C for 3 hours;

[0091] 4) The granules were taken out and granulated, dried at 60° C. to constant weight, crushed, and sieved to obtain white granular acrylamide polymer J4.

[0092] According to the calculation determined by the feed amount, based on the total weight of the acrylamide polymer J4, the content of the structural unit A is 90 weight %, the content of the structural unit B is 5 weight % and the content of the structural unit C is 5 weight %.

[0093] Example 5

[0094] An acrylamide polymer was prepared according to the method of Example 1, except that methacrylamide was used instead of acrylamide to obtain an acrylamide polymer J5.

[0095] According to the calculation determined by the feed amount, based on the total weight of the acrylamide polymer J5, the content of the structural unit A is 80 weight %, the content of the structural unit B is 15 weight % and the content of the structural unit C is 5 weight %.

[0096] Example 6

[0097] An acrylamide polymer was prepared according to the method of Example 1, except that monomer X2 was used instead of monomer X2 to obtain acrylamide polymer J6.

[0098] According to the calculation determined by the feed amount, based on the total weight of the acrylamide polymer J6, the content of the structural unit A is 80 weight %, the content of the structural unit B is 15 weight % and the content of the structural unit C is 5 weight %.

[0099] Example 7

[0100] An acrylamide polymer was prepared according to the method of Example 1, except that monomer Y2 was used instead of monomer Y1 to obtain acrylamide polymer J7.

[0101] According to the calculation determined by the feed amount, based on the total weight of the acrylamide polymer J7, the content of the structural unit A is 80 weight %, the content of the structural unit B is 15 weight % and the content of the structural unit C is 5 weight %.

[0102] Comparative Example 1

[0103] An acrylamide polymer was prepared according to the method of Example 1, except that an equal mass of monomer X was used instead of monomer Y to obtain an acrylamide polymer D1.

[0104] According to the calculation determined by the feed amount, based on the total weight of the acrylamide polymer D1, the content of the structural unit A is 80 weight %, the content of the structural unit B is 20 weight % and the content of the structural unit C is 0 weight %.

[0105] Comparative Example 2

[0106] An acrylamide polymer was prepared according to the method of Example 1, except that an equal mass of monomer Y was used instead of monomer X to obtain an acrylamide polymer D2.

[0107] According to the calculation determined by the feed amount, based on the total weight of the acrylamide polymer D2, the content of the structural unit A is 80 weight %, the content of the structural unit B is 0 weight % and the content of the structural unit C is 20 weight %.

[0108] Comparative Example 3

[0109] Acrylamide polymer was prepared according to the method of Example 1, except that the amount of acrylamide used was 216 g, the amount of monomer X1 used was 60 g, and the amount of monomer Y1 used was 24 g, to obtain acrylamide polymer D3.

[0110] According to the calculation determined by the feed amount, based on the total weight of the acrylamide polymer D3, the content of the structural unit A is 72 weight %, the content of the structural unit B is 20 weight % and the content of the structural unit C is 8 weight %.

[0111] Test Case

[0112] The acrylamide polymers obtained in the examples and comparative examples were respectively prepared into 0.15 wt % aqueous solutions, and the apparent viscosity, surface tension and interfacial tension of each aqueous solution were measured. The test results are shown in Table 1.

[0113] The apparent viscosity of the acrylamide polymer aqueous solution was measured by a Brookfield viscometer, the test temperature was 100°C, and the mineralization was 48000 mg / L;

[0114] The surface tension of acrylamide polymer aqueous solution in pure water was measured by DCAT-21 surface tension meter at a test temperature of 25°C;

[0115] The interfacial tension of the acrylamide polymer aqueous solution was measured by a TX500C interfacial tension meter from the American Kono Company. The test temperature was 100°C and the experimental oil was crude oil from Shengli Oilfield.

[0116] Table 1

[0117]

[0118]

[0119] It can be seen from the results in Table 1 that the acrylamide polymer provided by the present invention has a higher apparent viscosity under the conditions of a temperature of 100° C. and a mineralization of 48000 mg / L, showing excellent high temperature and high salt resistance; at the same time, it has lower surface tension and interfacial tension, showing excellent surface activity.

[0120] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing acrylamide polymer, characterized in that: The method comprises: (1) subjecting a monomer mixture to a solution polymerization reaction in water under solution polymerization reaction conditions and in the presence of an initiator to obtain a polymer colloid; wherein the monomer mixture comprises (meth)acrylamide, a monomer X and a monomer Y, wherein the monomer X has a structure represented by formula (4), and the monomer Y has a structure represented by formula (5); Based on the total amount of the monomer mixture, the amount of acrylamide is 80-90% by weight, the amount of the monomer X is 5-15% by weight, and the amount of the monomer Y is 1-5% by weight; (2) subjecting the polymer colloid to a hydrolysis reaction to obtain an acrylamide polymer; Wherein, R2' and R3' are each independently H or CH3, and R4' is methyl or ethyl.

2. The method according to claim 1, wherein: The conditions of the solution polymerization reaction include: the initiator is an oxidation-reduction system initiator; the reaction temperature is 10-20° C., the reaction time is 8-10 hours, and the pH value is 6-8.

3. The method according to claim 1, wherein: The conditions of the solution polymerization reaction also include: being carried out under an inert atmosphere.

4. The method according to claim 1, wherein: The amount of the initiator used is 0.015-0.15 parts by weight relative to 100 parts by weight of the monomer mixture.

5. The method according to claim 2, wherein: The oxidation-reduction system initiator is a persulfate oxidant and a sulfite reducer.

6. The method according to claim 5, wherein: Relative to 100 parts by weight of the monomer mixture, the persulfate oxidizing agent is 0.01-0.1 parts by weight; and the sulfite reducing agent is 0.005-0.05 parts by weight.

7. The method according to any one of claims 1 to 6, wherein: The conditions of the solution polymerization reaction also include: being carried out in the presence of a complexing agent, urea and a promoter.

8. The method according to claim 7, wherein: Relative to 100 parts by weight of the monomer mixture, the complexing agent is 0.01-0.1 parts by weight, the urea is 0.5-5 parts by weight, and the accelerator is 0.05-0.5 parts by weight.

9. The method according to claim 7, wherein: The complexing agent is disodium ethylenediaminetetraacetate, and the accelerator is 1,3-bis(4-methoxyphenyl)thiourea.

10. Acrylamide polymer obtained by the method according to any one of claims 1 to 9.

11. Use of the acrylamide polymer according to claim 10 as a displacement agent in an oil field.