A spinel ferrite hollow fiber and preparation method thereof
Through the sol-gel method and glass flat drawing technology, combined with the segmented heat treatment process, spinel ferrite hollow fibers are prepared, which solves the problems of complex processes and high sintering temperatures in the existing technology, and achieves high purity and good absorption. Material preparation with wave properties simplifies the process and reduces the sintering temperature.
Patent Information
- Application Number
- CN202211513086.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-11-29
AI Technical Summary
In the existing technology, the preparation method of spinel ferrite fiber has problems such as complex process, difficult to control conditions, high sintering temperature, etc., which affects the material performance, and there are difficulties in process operation and complexity of equipment.
The sol-gel method is combined with the glass flat drawing and segmented heat treatment process to form a precursor solution through metal salt and polymer solution, which is dried and sintered. The sintering temperature is controlled between 195 and 750°C, and the metal salt is adjusted. ratio and high molecular polymer concentration to prepare spinel ferrite hollow fibers.
It achieves high purity, good hysteresis loss and wave absorption performance of spinel ferrite hollow fibers, simplifies the process flow, reduces the sintering temperature, improves the formability of the material and the feasibility of industrial production.
Smart Images

Figure CN115679479B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of magnetic material preparation, and in particular to a spinel ferrite hollow fiber and a preparation method thereof. Background Art
[0002] With the development of science and technology, more and more electronic devices are used in people's lives, and the electromagnetic pollution generated is also increasing day by day. In the use of various high-precision information instruments and equipment, electromagnetic pollution often affects the operation of the equipment, and excessive high-frequency electromagnetic pollution may even cause long-term harm to human health. Absorbing materials can effectively reduce or eliminate electromagnetic pollution and thus become a research hotspot for experts and scholars from various countries. Ferrite absorbing materials have high resistivity and high-frequency magnetic permeability, and their main mechanism of absorbing electromagnetic wave energy is hysteresis loss, eddy current loss, ferromagnetic resonance, etc.
[0003] Ferrite itself is a ferromagnetic material. According to different structures, ferrite can be divided into three categories: spinel type, garnet type and magnetoplumbite type. All three types of ferrite can be used in the field of wave absorption. Among them, spinel ferrite fiber has both strong magnetic and dielectric properties, and its saturation magnetization intensity is much greater than the other two types of ferrite. In addition, its structural characteristics are conducive to wave absorption.
[0004] Among spinel ferrites, the typical representative nickel-zinc ferrite is widely used in instrumentation, radar, electronic countermeasures and other fields because of its advantages such as wide bandwidth, light weight and small size. The change of size and morphology of conventional micron-sized ferrites into nano-ferrites or hollow ferrites will reduce the overall specific gravity of the ferrite, and will also affect the electrical, magnetic, optical and other physical properties of the material itself, and ultimately have a certain impact on the performance of the material. Ferrite fiber materials are lighter in weight than powder and film materials, and their unique shape can solve the problem of nanoparticle agglomeration, which is conducive to reducing the weight of the coating and expanding the absorption band of electromagnetic waves.
[0005] Chinese patent ZL 201410314978.5 discloses a template method for preparing nickel-zinc ferrite materials, which uses metal nitrate as raw material and cotton fiber as template, without adding precipitant, etc., and is prepared in one step by solvent thermal method, replicating the microscopic morphology of cotton fiber, having good crystallization performance and magnetic properties, thereby effectively expanding the application range of nickel-zinc ferrite nanomaterials. However, this method is time-consuming and the obtained ferrite fiber structure is incomplete, and the sample morphology has a certain influence on the magnetic properties. Chinese patent ZL 200510095475.4 discloses a method for preparing spinel ferrite fiber by sol-gel method, which uses zinc nitrate, ferric nitrate and citric acid as raw materials, adjusts the pH value to 5.7 by adding ammonia water, dehydrates, draws and spins, dries, and sintered at 800-1000°C to obtain spinel zinc ferrite fiber with excellent performance. However, this method requires adjusting the pH value of the gel and the viscosity of the precursor at the same time, which increases the difficulty of process operation, and the precursor still needs to be sintered at a higher temperature to obtain ferrite fiber. Chinese patent ZL 201611154343.9 provides a method of utilizing a spinnable precursor solution containing a ceramic precursor, a polymer and a solvent, stretching the precursor solution into nanofibers by airflow, and collecting the nanofibers with a porous collector; sintering the collected nanofibers to obtain ceramic nanofibers. The obtained ceramic nanofibers have the characteristics of being ultra-light and resistant to high temperatures, and can be effectively used in many key and important fields. However, the method requires complex equipment, and there are problems such as difficulty in fiber collection due to solvent evaporation, needle blockage, and droplet formation.
[0006] Due to the characteristics of magnetic materials themselves, their preparation methods have problems such as complex processes, difficult to control conditions, and high calcination temperatures. The purpose of the present invention is to provide a preparation method with economical raw materials, simple process conditions, low sintering temperature, and is green and environmentally friendly. Summary of the invention
[0007] The purpose of the present invention is to solve the above problems in the prior art and to provide a spinel ferrite hollow fiber material with good hysteresis loss and wave absorption performance and a preparation method thereof. The method has the characteristics of simple preparation process, high purity of ferrite sample, and low reaction sintering temperature.
[0008] In order to achieve the above object, the present invention adopts the following technical scheme:
[0009] A method for preparing a spinel ferrite hollow fiber comprises the following steps:
[0010] 1) dissolving a metal iron salt and two or more second metal salts in an organic solvent to obtain a metal salt mixed solution, adding a polymer to anhydrous ethanol and stirring evenly to obtain a polymer solution, adding the metal salt mixed solution to the polymer solution, and continuously stirring to obtain a precursor solution;
[0011] 2) The precursor solution in step 1) is drawn using a glass plate at a certain humidity to obtain an organogel fiber, and hot air is used to assist in drying to remove part of the solvent, and then the organogel fiber is collected and placed in an oven for drying;
[0012] 3) placing the organic gel fiber dried in step 2) into a tubular furnace for sintering by a staged heat treatment process to obtain spinel ferrite hollow fibers.
[0013] The second metal salt may be two or more of chlorides, sulfates, nitrates, perchlorates, carbonates, and acetylacetonates of nickel, cobalt, zinc, manganese, iron, calcium, titanium, aluminum, lithium, copper, vanadium, and chromium, and the metal of the second metal salt is preferably nickel and zinc.
[0014] The metal iron salt may be one of ferric chloride, ferric nitrate, ferric sulfate, ferric perchlorate, ferric carbonate, and ferric acetylacetonate.
[0015] The organic solvent is N,N-dimethylformamide (DMF), tetrahydrofuran (THF) or dimethyl carbonate (DMC); the high molecular polymer is polyvinyl pyrrolidone (PVP), polyacrylonitrile (PAN), polyethylene oxide (PEO) or polyvinylidene fluoride (PVDF).
[0016] The molar ratio of the trivalent iron ions of the metallic iron salt to the total second metal ions is 2:1.
[0017] In the metal salt mixed solution, the total mass fraction of the metal iron salt and the second metal salt is 20wt.% to 30wt.%.
[0018] In the high molecular polymer solution, the mass fraction of the high molecular polymer is 20wt.% to 25wt.%.
[0019] In step 2), the humidity is lower than 70%.
[0020] The segmented heat treatment process in step 3) is as follows: the organogel fiber is pre-oxidized at 195-220°C in an air atmosphere for 120 minutes, then heated to 450-750°C for 120 minutes, and then taken out after cooling to room temperature in the furnace; the heating rate is 2-4°C / min, and the flow rate is 60-120mL / min.
[0021] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0022] (1) The spinel ferrite hollow fiber prepared by the present invention has good hysteresis loss and wave absorption performance, and is expected to be applied to wave absorbing coating materials. Due to the characteristics of the hollow fiber structure, the requirements of "light and thin" of the wave absorbing coating material can be improved, and the internal multiple attenuation reflection can be increased to improve the electromagnetic wave absorption effect.
[0023] (2) The spinel ferrite hollow fibers prepared by the present invention have good formability, a diameter between 0.5 and 2 μm, a low volume density, and a uniform and dense microstructure;
[0024] (3) The process of the present invention is simple and economical. The morphology and structure of the fiber can be controlled by adjusting technical parameters such as the ratio of metal salts / mass concentration of PVP / sintering temperature, which is convenient for promotion to realize industrial production. Specifically, the addition ratio of metal salts directly affects the integrity of the hollow shell formed by the spinel ferrite hollow fiber and its magnetic properties; the adjustment of the mass concentration of PVP can control the viscosity of the precursor, and the viscosity affects the diameter of the fiber; the adjustment of the sintering temperature lies in the selection of a low-temperature calcination part slightly higher than the glass transition temperature of PVP (Tg = 180°C), so that the PVP macromolecules can move more freely, and the precursor diffuses through the polymer chain to form a shell. In the high-temperature stage, PVP is completely decomposed to finally form a spinel ferrite hollow fiber structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the infrared (FT-IR) spectrum of the spinel ferrite hollow fiber prepared in Examples 1 to 4.
[0026] Figure 2 X-ray diffraction (XRD) patterns of the spinel ferrite hollow fibers prepared in Examples 1-4.
[0027] Figure 3 It is the VSM spectrum of the spinel ferrite hollow fiber prepared in Examples 1 to 4.
[0028] Figure 4 This is a scanning electron microscope (SEM) image of the surface of the spinel ferrite hollow fiber ceramic prepared in Examples 1 to 4. Figure 4 In the present invention, (a) the spinel ferrite hollow fiber prepared in Example 1 is sintered at 450°C; (b) the spinel ferrite hollow fiber prepared in Example 2 is sintered at 550°C; (c) the spinel ferrite hollow fiber prepared in Example 3 is sintered at 650°C; (d) the spinel ferrite hollow fiber prepared in Example 4 is sintered at 750°C. DETAILED DESCRIPTION
[0029] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention clearer and more understandable, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0030] Example 1
[0031] 1. Dissolve 0.578 g of NiCl2·6H2O, 0.220 g of ZnCl2 and 3.268 g of Fe(NO3)3·9H2O in 10 mL of DMF in sequence, where the mass fraction of the metal salt is 30%, and disperse the mixed solution by ultrasonication for 20 min;
[0032] 2. Place 20 mL of anhydrous ethanol in a magnetic stirrer and stir at 30 rpm at room temperature, and slowly and evenly add 4.50 g of PVP into the anhydrous ethanol, wherein the mass fraction of polyvinyl pyrrolidone is 22%, and continue stirring for 2 h to obtain a viscous solution;
[0033] 3. Add the mixed solution of DMF and metal salt into the PVP / anhydrous ethanol solution, adjust the speed of the magnetic stirrer to 60 rpm and continue stirring for 3 hours to obtain a uniform and transparent yellow-brown precursor solution;
[0034] 4. In a room temperature environment with an air humidity below 70%, the organogel fibers were drawn using parallel glass plates, and 60°C hot air was used for auxiliary drying to remove part of the solvent. The organogel fibers were then collected in a culture dish and placed in an oven for heating and drying at 80°C for 5 hours to fully remove the organic solvent.
[0035] 5. Put the organic gel fiber obtained by drying into a tubular furnace and carry out low-temperature pre-oxidation at 200°C for 120 minutes, then raise the temperature to 450°C and keep it for 120 minutes, and finally cool it to room temperature with the furnace and take it out to obtain spinel ferrite hollow fiber; the sintering atmosphere is air, the heating rate is 3°C / min, and the flow rate is preferably 60mL / min.
[0036] Example 2
[0037] 1. Dissolve 0.578 g of NiCl2·6H2O, 0.220 g of ZnCl2 and 3.268 g of Fe(NO3)3·9H2O in 10 mL of DMF in sequence, where the mass fraction of the metal salt is 30%, and disperse the mixed solution by ultrasonication for 20 min;
[0038] 2. Place 20 mL of anhydrous ethanol in a magnetic stirrer and stir at 30 rpm at room temperature, and slowly and evenly add 4.50 g of PVP into the anhydrous ethanol, wherein the mass fraction of polyvinyl pyrrolidone is 22%, and continue stirring for 2 h to obtain a viscous solution;
[0039] 3. Add the mixed solution of DMF and metal salt into the PVP / anhydrous ethanol solution, adjust the speed of the magnetic stirrer to 60 rpm and continue stirring for 3 hours to obtain a uniform and transparent yellow-brown precursor solution;
[0040] 4. In a room temperature environment with an air humidity below 70%, the organogel fibers were drawn using parallel glass plates, and 60°C hot air was used for auxiliary drying to remove part of the solvent. The organogel fibers were then collected in a culture dish and placed in an oven for heating and drying at 80°C for 5 hours to fully remove the organic solvent.
[0041] 5. Put the organic gel fiber obtained by drying into a tubular furnace and carry out low-temperature pre-oxidation at 200°C for 120 minutes, then raise the temperature to 550°C and keep it for 120 minutes, and finally cool it to room temperature with the furnace and take it out to obtain spinel ferrite hollow fiber; the sintering atmosphere is air, the heating rate is 3°C / min, and the flow rate is preferably 60mL / min.
[0042] Example 3
[0043] 1. Dissolve 0.578 g of NiCl2·6H2O, 0.220 g of ZnCl2 and 3.268 g of Fe(NO3)3·9H2O in 10 mL of DMF in sequence, where the mass fraction of the metal salt is 30%, and disperse the mixed solution by ultrasonication for 20 min;
[0044] 2. Place 20 mL of anhydrous ethanol in a magnetic stirrer and stir at 30 rpm at room temperature, and slowly and evenly add 4.50 g of PVP into the anhydrous ethanol, wherein the mass fraction of polyvinyl pyrrolidone is 22%, and continue stirring for 2 h to obtain a viscous solution;
[0045] 3. Add the mixed solution of DMF and metal salt into the PVP / anhydrous ethanol solution, adjust the speed of the magnetic stirrer to 60 rpm and continue stirring for 3 hours to obtain a uniform and transparent yellow-brown precursor solution;
[0046] 4. In a room temperature environment with an air humidity below 70%, the organogel fibers were drawn using parallel glass plates, and 60°C hot air was used for auxiliary drying to remove part of the solvent. The organogel fibers were then collected in a culture dish and placed in an oven for heating and drying at 80°C for 5 hours to fully remove the organic solvent.
[0047] 5. Put the organic gel fiber obtained by drying into a tubular furnace and carry out low-temperature pre-oxidation at 200°C for 120 minutes, then raise the temperature to 650°C and keep it for 120 minutes, and finally cool it to room temperature with the furnace and take it out to obtain spinel ferrite hollow fiber; the sintering atmosphere is air, the heating rate is 3°C / min, and the flow rate is preferably 60mL / min.
[0048] Example 4
[0049] 1. Dissolve 0.578 g of NiCl2·6H2O, 0.220 g of ZnCl2 and 3.268 g of Fe(NO3)3·9H2O in 10 mL of DMF in sequence, where the mass fraction of the metal salt is 30%, and disperse the mixed solution by ultrasonication for 20 min;
[0050] 2. Place 20 mL of anhydrous ethanol in a magnetic stirrer and stir at 30 rpm at room temperature, and slowly and evenly add 4.50 g of PVP into the anhydrous ethanol, wherein the mass fraction of polyvinyl pyrrolidone is 22%, and continue stirring for 2 h to obtain a viscous solution;
[0051] 3. Add the mixed solution of DMF and metal salt into the PVP / anhydrous ethanol solution, adjust the speed of the magnetic stirrer to 60 rpm and continue stirring for 3 hours to obtain a uniform and transparent yellow-brown precursor solution;
[0052] 4. In a room temperature environment with an air humidity below 70%, the organogel fibers were drawn using parallel glass plates, and 60°C hot air was used for auxiliary drying to remove part of the solvent. The organogel fibers were then collected in a culture dish and placed in an oven for heating and drying at 80°C for 5 hours to fully remove the organic solvent.
[0053] 5. Put the organic gel fiber obtained by drying into a tubular furnace and carry out low-temperature pre-oxidation at 200°C for 120 minutes, then raise the temperature to 750°C and keep it for 120 minutes, and finally cool it to room temperature with the furnace and take it out to obtain spinel ferrite hollow fiber; the sintering atmosphere is air, the heating rate is 3°C / min, and the flow rate is preferably 60mL / min.
[0054] The infrared (FT-IR) spectrum of the spinel ferrite hollow fiber of the present invention ( Figure 1 ) showed that all samples contained 570 cm -1 The absorption band near is caused by the vibration between the metal ions and oxygen ions on the tetrahedral A position, which can prove that this method can form the spinel ferrite phase at a low temperature stage (450°C). The X-ray diffraction (XRD) diagram of the spinel ferrite hollow fiber of the present invention ( Figure 2) has multiple characteristic peaks of spinel ferrite, among which 2θ=29.5° / 35.1° / 42.8° / 56.9° / 62.4° correspond to the (220) / (311) / (400) / (511) / (440) crystal planes of spinel ferrite, respectively. As the temperature rises, the diffraction peak intensity gradually increases. The VSM spectrum of the spinel ferrite hollow fiber of the present invention is as follows: Figure 3 As shown, the hysteresis loop of the sample is in a saturated state, and its magnetic saturation intensity gradually increases with the increase of temperature. The scanning electron microscope (SEM) image of the spinel ferrite hollow fiber of the present invention is as follows: Figure 4 As shown, the ferrite fiber is a hollow fiber with good integrity, a smooth and dense surface, and a fiber diameter ranging from 0.5 to 2 μm.
[0055] The present invention adopts a sol-gel method and a flat spinning and pulling technology to prepare a continuous spinel ferrite hollow fiber, which improves the manufacturing cost and the safety of spinning. At the same time, no change in the valence state of metal ions occurs during the reaction process, so that the purity of the product is high. Polyvinyl pyrrolidone / anhydrous ethanol solution is used as a precursor, and Fe is reacted in a liquid phase. 3+ , Ni 2+ , Zn 2+ The mixture is uniformly mixed, and ferrite is generated on the surface with polyvinyl pyrrolidone as the skeleton in the low-temperature pre-oxidation stage, and the polyvinyl pyrrolidone is removed at high temperature to obtain hollow ferrite fibers. The hollow ferrite fibers are used as absorbing materials to improve the overall absorbing performance while reducing the overall mass, or the fibers are spread on the outer layer of the material in the form of a coating to improve its electromagnetic wave attenuation ability through multiple attenuation reflections, which has great application value in radar, stealth materials, and electromagnetic shielding.
Claims
1. A method for preparing a spinel ferrite hollow fiber, characterized in that The following steps are involved: 1) Dissolving a metal iron salt and two or more second metal salts in an organic solvent to obtain a metal salt mixed solution, adding a polymer to anhydrous ethanol and stirring evenly to obtain a polymer solution, adding the metal salt mixed solution to the polymer solution, and continuously stirring to obtain a precursor solution; in the metal salt mixed solution, the total mass fraction of the metal iron salt and the second metal salt is 20wt.%~30wt.%, and the organic solvent is 70wt.%~80wt.%; in the polymer solution, the mass fraction of the polymer is 20wt.%~25wt.%; 2) The precursor solution in step 1) is drawn using a glass plate at a certain humidity to obtain an organogel fiber, and hot air-assisted drying is used to remove part of the solvent, and then the organogel fiber is collected and placed in an oven for drying; 3) The dried organic gel fiber is placed in a tubular furnace for sintering by a staged heat treatment process. Specifically, the organic gel fiber is pre-oxidized and kept at 195-220°C in an air atmosphere for 120 minutes, then heated to 450-750°C and kept for 120 minutes, and then taken out after cooling to room temperature with the furnace; the heating rate is 2-4°C / min, and the air flow rate is 60-120mL / min to obtain spinel ferrite hollow fibers.
2. The method for preparing a spinel ferrite hollow fiber according to claim 1, characterized in that: The second metal salt is selected from chlorides, sulfates, nitrates, perchlorates, carbonates, and acetylacetonates of nickel, cobalt, zinc, manganese, iron, calcium, titanium, aluminum, lithium, copper, vanadium, and chromium.
3. The method for preparing a spinel ferrite hollow fiber according to claim 2, characterized in that: The metals of the second metal salt are nickel and zinc.
4. The method for preparing a spinel ferrite hollow fiber according to claim 1, characterized in that: The metal iron salt is one of ferric chloride, ferric nitrate, ferric sulfate, ferric perchlorate, ferric carbonate and ferric acetylacetonate.
5. The method for preparing a spinel ferrite hollow fiber according to claim 1, characterized in that: The organic solvent is N,N-dimethylformamide, tetrahydrofuran or dimethyl carbonate; the high molecular polymer is polyvinyl pyrrolidone, polyacrylonitrile, polyethylene oxide or polyvinylidene fluoride.
6. The method for preparing a spinel ferrite hollow fiber according to claim 1, characterized in that: The molar ratio of the trivalent iron ions of the metallic iron salt to the total second metal ions is 2:
1.
7. The method for preparing a spinel ferrite hollow fiber according to claim 1, characterized in that: In step 2), the humidity is lower than 70%.
8. The spinel ferrite hollow fiber prepared by the preparation method according to any one of claims 1 to 7.
Citation Information
Patent Citations
Preparation method of nickel ferrite magnetic nanofiber material
CN104045336A
Ceramic nanofiber and preparing method and device thereof
CN106637446A
Ni-Zn ferrite fibre and preparing process thereof
CN101100374A
Ni-Zn ferrite / SiO2 composite nano-fiber and preparation method thereof
CN101914821A
Li-Zn ferrite magnetic nanofibers and their preparation methods
CN102286805A