A method for preparing micron-sized particle cross-sections that can be repeatedly used for electron microscope observation

By using conductive metal sheets and cold mounting solutions to fix and cover the powder to be observed, combined with mold and grinding technology, the problems of high equipment, high cost and oxidation failure in the existing technology are solved, and low-cost, repeatable micron-level measurements are achieved. Particle cross-section preparation and observation.

CN115684229BActive Publication Date: 2024-10-29HARBIN INST OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211153574.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-21
Publication Date
2024-10-29
Estimated Expiration
2042-09-21

AI Technical Summary

Technical Problem

When preparing cross-sections of micron-sized particles using the existing technology, the equipment requirements are high, the cost is high, and the samples are disposable, making it difficult to achieve repeated observations. In particular, the treatment of temperature-sensitive materials will destroy their original organizational structure and be greatly affected by oxidation failure.

Method used

Use a conductive metal sheet and cold mounting solution (polymethylmethacrylate and metallographic epoxy curing agent) to fix and cover the powder to be observed, remove the mold and then polish it to obtain a reusable particle cross-section, using the bending section and the test section The angle design facilitates grinding and observation and reduces oxidation failure.

Benefits of technology

It achieves low-cost, repeatable preparation of micron-level particle cross-sections, has strong operability, can observe cross-sections at different depths, reduces the impact of oxidation failure, and is suitable for electron microscopy observation of temperature-sensitive materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003857358400000011
    Figure HDA0003857358400000011
  • Figure HDA0003857358400000012
    Figure HDA0003857358400000012
  • Figure HDA0003857358400000021
    Figure HDA0003857358400000021
Patent Text Reader

Abstract

The present invention belongs to the technical field of scanning electron microscope sample preparation, and relates to a method for preparing a micron-level particle cross section that can be repeatedly used for electron microscope observation, comprising the following steps: step 1: spreading the powder to be observed on the powder test section to be observed of a conductive metal sheet; step 2: using a cold embedding solution to completely cover the powder to be observed on the conductive metal sheet; step 3: waiting for the cold embedding solution to fix the powder to be observed on the conductive metal sheet; step 4: putting the conductive metal sheet into a mold, filling the mold with a cold embedding solution, vertically extending one end of the bent section of the conductive metal sheet out of the cold embedding solution, and facing the side with the powder to be observed toward the bottom of the mold; step 5: demolding after the cold embedding solution in the mold is solidified, grinding the covering area containing the powder to be observed, and obtaining the particle cross section for scanning electron microscope observation. The method does not require any equipment and has low cost; the sample that is easy to oxidize can be reused after one sample preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of scanning electron microscope sample preparation, and relates to a method for preparing a micron-level particle cross section which can be repeatedly used for electron microscope observation. Background Art

[0002] In the process of material development and research, especially nanomaterials, the characterization of their internal microstructure is an indispensable means. When characterizing the microstructure and morphology of spherical particles, it is easy to analyze their surface, but it is not easy to prepare samples when characterizing their internal organization and structure. Focused ion beam cutting, slicing, and ion beam polishing can be used to prepare relatively ideal internal cross-sections, but these methods obtain a small number of cross-sections, have high equipment requirements, and are difficult to promote due to high costs. Moreover, the samples are disposable samples and need to be re-sampled after being exposed to oxidation in the air. The conductive hot embedding method can obtain the internal cross-section of material particles at a lower cost and faster speed, but for some materials that have strict temperature requirements (such as nano hydrogen storage alloys), the heating process will destroy their original organizational structure, and it is difficult to ensure the authenticity of the cross-section. Summary of the invention

[0003] Purpose of the Invention

[0004] The present invention aims to solve the problems existing in the above cross-section sample preparation process and provides a method for preparing micron-level particle cross-sections that can be repeatedly used for electron microscope observation.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for preparing a micron-sized particle cross section that can be repeatedly used for electron microscope observation comprises the following steps:

[0007] Step 1: A conductive metal sheet is provided, wherein the conductive metal sheet includes a powder test section to be observed and a bending section, and the powder to be observed is spread flat on one side of the powder test section to be observed of the conductive metal sheet;

[0008] Step 2: Fill the spaces and cracks between the powders to be observed with a cold mounting solution and completely cover the conductive metal sheet, wherein the cold mounting solution includes polymethyl methacrylate CAS9011-14-7 and a metallographic epoxy curing agent;

[0009] Step 3: Fix the powder to be observed on the conductive metal sheet by cold mounting solution;

[0010] Step 4: Place the conductive metal sheet in step 3 into a mold with a cavity therein, fill the cavity in the mold with a cold mounting solution, extend one end of the bent section of the conductive metal sheet vertically out of the cold mounting solution, and place the side of the powder test section to be observed with the powder to be observed toward the bottom of the mold;

[0011] Step 5: After the cold mounting solution filled in the mold in step 4 is solidified, demolding is performed, and then the covering area containing the powder to be observed is polished to obtain a particle cross section for scanning electron microscopy observation.

[0012] As a further description of the above solution, the conductive metal sheet is a copper sheet or an aluminum sheet with a thickness of 0.2mm-0.5mm.

[0013] As a further description of the above solution, the mold is a square or cylindrical silicone soft mold.

[0014] As a further description of the above solution, the angle between the bending section and the powder test section to be observed is greater than or equal to 85° and less than 90° or greater than 90° and less than or equal to 95°.

[0015] As a further description of the above solution, the powder testing section to be observed is covered with powder to be observed, and the distance between the edge of the area covered by the powder to be observed and the bending section is 5-8 mm.

[0016] As a further description of the above scheme, the weight ratio of the polymethyl methacrylate CAS9011-14-7 to the metallographic epoxy curing agent is 1:(0.7-0.9).

[0017] As a further description of the above scheme, the polishing in step 5 includes:

[0018] Step A: Grind the demoulded conductive metal sheet with 800# sandpaper, 1200# sandpaper and 2000# sandpaper respectively until the powder to be observed is exposed;

[0019] Step B: Finely grind the powder to be observed in step A with 3000# sandpaper and 5000# sandpaper respectively to obtain the particle cross section of the powder to be observed.

[0020] A mold for making a specimen for electron microscope observation, comprising a mold, a first cover plate and a second cover plate;

[0021] The first cover plate includes a shell, a movable clamp and a clamp position adjustment bolt, the shell has a accommodating space inside and an opening on one side of the shell; the movable clamp is arranged in the accommodating space of the shell and is slidably connected to the inner wall of the shell; the clamp position adjustment bolt passes through the shell and is fixedly connected to the movable clamp, and the clamp position adjustment bolt is slidably connected to the shell; the bottom of the shell has an installation groove, and the installation groove is interference connected with the top of the mold; the second cover plate has the same structure as the first cover plate and is symmetrically arranged on the mold.

[0022] The micron-level powder to be observed of the present invention is arranged on one side of a conductive metal sheet through a cold embedding solution, and the conductive metal sheet arranged on one side of the powder to be observed is arranged obliquely to the bottom of the cold embedding solution after demoulding and solidification. Therefore, when it is necessary to observe the cross section of the powder to be observed by electron microscope, only a part of the particles covered by the cold embedding solution needs to be polished each time; if the cross section of the powder to be observed is to be observed next time, the other parts of the cross section of the powder to be observed covered by the cold embedding solution can be continued to be polished, so that it can be repeatedly used for electron microscope observation without the assistance of other equipment, has strong operability, and low sample preparation cost; the observable area is wide, and the cross sections of particles at different depths can be observed at the same time in one sample preparation; the influence of oxidation failure is small, and if the cross section fails due to oxidation, a part can be ground off and the same batch of powder to be observed can be continued to be observed. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the preparation of a micron-sized particle cross section that can be repeatedly used for electron microscopy observation;

[0024] Figure 2 is the Mg after high energy ball milling shown in Example 1 85 Ni 15 Particle cross-section of the alloy;

[0025] Figure 3 The Mg after hydrogenation shown in Example 2 85 Ni 14.8 Ag 0.2 A magnified cross-section of a particle of the alloy;

[0026] Figure 4 is the Mg shown in Example 3 85 Ni 14.8 Ag 0.2 Cross-section of a hydride particle after dehydrogenation;

[0027] Figure 5 Mg in Example 4 85 Ni 14.5 In 0.5 Cross-section of the alloy particles after high-energy ball milling;

[0028] Figure 6 It is semi-hydrogen absorbing Mg 85 Ni 14.6 Ag 0.4 A cross-section of a particle of the alloy.

[0029] Description of reference numerals:

[0030] Figure 1 In the figure: 1-conductive metal sheet; 2-cold mounting solution; 3-mold; 4-powder to be observed; 5-clamp position adjustment bolt; 6-shell, 7-movable clamp. DETAILED DESCRIPTION

[0031] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.

[0032] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0033] The components of the embodiments of the present invention generally described and shown in the drawings herein may be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention.

[0034] A method for preparing a micron-sized particle cross section that can be repeatedly used for electron microscope observation comprises the following steps:

[0035] Step 1: comprising a conductive metal sheet 1, wherein the conductive metal sheet 1 comprises a powder test section to be observed and a bending section, and the powder 4 to be observed is spread flat on one side of the powder test section to be observed of the conductive metal sheet 1, and the specific conductive metal sheet 1 is a copper sheet or aluminum sheet with a thickness of 0.2mm-0.5mm;

[0036] Step 2: Use a cold mounting solution 2 to fill the space and cracks between the powders 4 to be observed and completely cover them on the conductive metal sheet 1, wherein the cold mounting solution 2 includes polymethyl methacrylate CAS9011-14-7 and a metallographic epoxy curing agent, wherein the weight ratio of polymethyl methacrylate CAS9011-14-7 to the metallographic epoxy curing agent is 1:(0.7-0.9), wherein the main components of the metallographic epoxy curing agent are isophorone diamine, benzoic acid, trimethylcyclohexane dicarboxylic acid and 2,4,6-triphenol; this method can completely cover the powders 4 to be observed with the cold mounting material 2 to isolate the air and fix them on the conductive metal sheet 1, so that the bombarding electrons during observation are conducted away through the conductive metal sheet 1;

[0037] Step 3: The cold mounting solution 2 fixes the powder 4 to be observed on the conductive metal sheet 1;

[0038] Step 4: Place the conductive metal sheet 1 in step 3 into a mold 3 with a cavity inside, fill the cavity in the mold 3 with a cold embedding solution 2, extend one end of the bent section of the conductive metal sheet 1 vertically out of the cold embedding solution 2, and place the side of the powder test section to be observed with the powder 4 to be observed toward the bottom of the mold 3; since the conductive metal sheet 1 is a copper sheet or aluminum sheet with a thickness of 0.2mm-0.5mm, it is not convenient to repeatedly polish it, nor is it convenient to place it on an electron microscope for observation. Therefore, in step 4, the conductive metal sheet 1 is made into a structure that is easy to polish and observe with an electron microscope with a cold embedding solution 2, so that the subsequent polishing and electron microscope observation are easier. Step 5: After the cold embedding solution 2 is solidified, demold it, and then polish the covering area containing the powder 4 to be observed to obtain a particle cross section for scanning electron microscope observation.

[0039] Step 5: After the cold mounting solution 2 filled in the mold in step 4 is solidified, demolding is performed, and then the covering area containing the powder 4 to be observed is polished to obtain a particle cross section for scanning electron microscopy observation.

[0040] The micron-scale powder to be observed 4 of the present application is set on one side of the conductive metal sheet 1 through the cold embedding solution 2, and the conductive metal sheet 1 on one side of the powder to be observed 4 is set at an angle to the bottom of the cold embedding solution 2 after demolding and curing. Therefore, when it is necessary to observe the cross section of the powder to be observed by electron microscopy, only a part of the particle cross section of the powder to be observed 4 covered by the cold embedding solution needs to be polished each time; if the next observation is made, the particle cross section of the powder to be observed 4 that is covered by the cold embedding solution can continue to be polished, so that it can be repeatedly used for electron microscopy observation without the assistance of other equipment, with strong operability and low sample preparation cost; the observable area is wide, and the cross sections of particles at different depths can be observed simultaneously in one sample preparation; it is less affected by oxidation failure. If the cross section fails due to oxidation, a part can be ground off and the same batch of powder to be observed 4 can continue to be observed.

[0041] The conductive metal sheet 1 in the embodiment of the present invention is a copper sheet or an aluminum sheet with a thickness of 0.2 mm to 0.5 mm.

[0042] The mold 3 in the embodiment of the present invention is a square or cylindrical silicone soft mold, which can be quickly demoulded after the powder 4 to be observed is solidified.

[0043] The conductive metal sheet 1 of the embodiment of the present invention includes a powder test section to be observed and a bending section, and the angle between the bending section and the powder test section to be observed is greater than or equal to 85° and less than 90° or greater than 90° and less than or equal to 95°; the angle between the bending section and the powder test section to be observed in the present application can ensure that the powder test section to be observed is inclined with the bottom of the cold-embedded material 2 after demolding, so each time sandpaper is used for grinding, only particles in a part of the area can be ground, and a new cross-section of the powder 4 to be observed can continue to be ground for the next observation, so that it can be repeatedly used for electron microscopy observation; at the same time, the angle between the bending section and the powder test section to be observed cannot be 90°, because this will grind all the powder 4 to be observed at once during the grinding process, resulting in the inability to be repeatedly used for electron microscopy observation, and can only be re-sampled.

[0044] The powder test section to be observed in the embodiment of the present invention is covered with powder 4 to be observed, and the distance between the edge of the area covered by the powder 4 to be observed and the bending section is 5-8 mm. This setting can ensure that the powder 4 to be observed is all in the powder test section to be observed, preventing the covered powder 4 to be observed from falling off.

[0045] The inner diameter of the mold 3 in the embodiment of the present invention is 18-25 mm, and the size of the conductive metal sheet 1 is 4 mm×20 mm.

[0046] The polishing in step 5 above includes:

[0047] Step A: Grind the conductive metal sheet 1 covered with the powder 4 to be observed with 800# sandpaper, 1200# sandpaper and 2000# sandpaper respectively, or grind with 400# sandpaper, 1000# sandpaper, 1500# sandpaper and 2000# sandpaper until the conductive metal sheet 1 is exposed;

[0048] Step B: Use 3000# sandpaper and 5000# sandpaper to perform fine sanding to reduce scratches and obtain a relatively smooth cross-section.

[0049] A mold for making a specimen for electron microscope observation, comprising a mold 3, a first cover plate and a second cover plate;

[0050] The first cover plate includes a housing 6, a movable clamping plate 7 and a clamping plate position adjustment bolt 5, wherein the housing 6 has a receiving space inside and an opening on one side of the housing 6; wherein the movable clamping plate 7 is arranged in the receiving space of the housing 6 and is slidably connected to the inner wall of the housing 6; wherein the clamping plate position adjustment bolt 5 passes through the housing 6 and is fixedly connected to the movable clamping plate 7, and the clamping plate position adjustment bolt 5 is slidably connected to the housing 6; the bottom of the housing 6 has a mounting groove, and the mounting groove is interference-connected with the top of the mold 3; the second cover plate has the same structure as the first cover plate and is symmetrically arranged on the mold 3. This structure can clamp and fix the conductive metal sheet 1 in the mold 3 by the first cover plate and the second cover plate, and the operator does not need to support the conductive metal sheet 1 by hand to ensure the position of the conductive metal sheet 1, and after the cold mounting solution 2 is solidified, the cover plate can be removed for demoulding, and the structure is simple and convenient to operate. Example

[0051] Preparation of Mg after high energy ball milling 85 Ni 15 The cross section of the alloy micron-sized particles is obtained by ball milling in a planetary high-energy ball mill. The process parameters of the ball milling are: ball-to-material ratio 30:1, rotation speed 280 rpm, and ball milling time 2 hours. The implementation effect of the invention using this technical method is as follows Figure 2 As shown in the figure, the cross-section of the prepared particles is clear, the particles are complete, and the pores inside the particles are clearly visible. It can be clearly observed that Mg 85 Ni 15 There are two structures in the alloy, namely the bright white Mg2Ni phase and the dark gray Mg phase. The Mg2Ni phase is randomly embedded in the Mg matrix.

[0052] The specific preparation process includes the following steps:

[0053] 1. The powder 4 to be observed after high-energy ball milling is evenly spread on one end of an aluminum sheet of 4mm×20mm in size, covering an area of ​​4mm×4mm. The aluminum sheet is bent 5mm away from the edge of the area covered by the powder 4 to make the angle between the bent section of the aluminum sheet and the test section of the powder to be observed 85°, presenting an approximate L-shape;

[0054] 2. The powder 4 to be observed is completely coated on the aluminum sheet with a cold mounting solution 2, wherein the cold mounting solution 2 comprises polymethyl methacrylate CAS9011-14-7 and a metallographic epoxy curing agent, wherein the weight ratio of polymethyl methacrylate CAS9011-14-7 to the metallographic epoxy curing agent is 1:0.7; wherein the main components of the metallographic epoxy curing agent are isophorone diamine, benzoic acid, trimethylcyclohexane dicarboxylic acid and 2,4,6-triphenol;

[0055] 3. After the cold mounting solution 2 fixes the powder 4 to be observed on the conductive metal sheet 1;

[0056] 4. Put the aluminum sheet into a mold 3 with a cavity inside, fill the cavity inside the mold 3 with the cold mounting solution 2, vertically extend the side of the aluminum sheet without the observed powder out of the cold mounting solution 2, and the side of the conductive metal sheet 1 provided with the observed powder 4 toward the bottom of the mold 3, and let it stand at room temperature for 20-30 minutes to solidify;

[0057] 5. After the cold mounting solution 2 solidifies, take out the sample and polish the side containing the powder 4 to be observed with 800# sandpaper, 1200# sandpaper and 2000# sandpaper respectively until the aluminum sheet is exposed. Finally, finely polish it with 3000# sandpaper and 5000# sandpaper respectively before use for scanning electron microscopy observation. Example

[0058] Preparation of hydrogenated Mg 85 Ni 14.8 Ag 0.2 Particle cross section, the observed particles are obtained from the powder after high-energy ball milling and hydrogenation treatment. The high-energy ball milling process is: ball-to-material ratio 30:1, rotation speed 280rpm, ball milling time 2.5h. The hydrogenation conditions are 275℃, 2.0MPa hydrogen atmosphere pressure for 1.5h. The implementation effect of the method of the present invention is as follows Figure 3 As shown, the internal structure of the alloy after hydrogenation can be seen, wherein the bright white particles are Mg2NiH4 phases and the gray particles are MgH2 phases. Even though the nano-Mg2NiH4 is randomly distributed in the hydrogen storage alloy particles so that the MgH2 phase is no longer continuous, the edges of the particles prepared by the method of the present invention are still intact.

[0059] The specific preparation process includes the following steps:

[0060] 1. The powder 4 to be observed after hydrogenation treatment is evenly spread on one end of an aluminum sheet of 4 mm × 20 mm in size, covering an area of ​​4 mm × 4 mm, and the aluminum sheet is bent downward at a distance of 5 mm from the edge of the area covered by the powder 4 to be observed, so that the angle between the bent section of the aluminum sheet and the test section of the powder to be observed is 89°, presenting an approximately L-shape;

[0061] 2. The powder 4 to be observed is completely coated on the aluminum sheet with a cold mounting solution 2, wherein the cold mounting solution 2 comprises polymethyl methacrylate CAS9011-14-7 and a metallographic epoxy curing agent, wherein the weight ratio of polymethyl methacrylate CAS9011-14-7 to the metallographic epoxy curing agent is 1:0.8; wherein the main components of the metallographic epoxy curing agent are isophorone diamine, benzoic acid, trimethylcyclohexane dicarboxylic acid and 2,4,6-triphenol;

[0062] 3. After the cold mounting solution 2 fixes the powder 4 to be observed on the conductive metal sheet 1;

[0063] 4. Put the aluminum sheet into a mold 3 with a cavity inside, fill the cavity inside the mold 3 with the cold mounting solution 2, vertically extend the side of the conductive metal sheet 1 without the observed powder out of the cold mounting solution 2, and the side of the aluminum sheet with the observed powder 4 faces the bottom of the mold 3, and let it stand at room temperature for 20-30 minutes to solidify;

[0064] 5. After the cold mounting solution 2 solidifies, take out the sample and polish the side containing the powder 4 to be observed with 800# sandpaper, 1200# sandpaper and 2000# sandpaper respectively until the aluminum sheet is exposed. Finally, finely polish it with 3000# sandpaper and 5000# sandpaper respectively before use for scanning electron microscopy observation. Example

[0065] Preparation of Mg 85 Ni 14.8 Ag 0.2 The cross section of the particles after the hydride is released. The observed particles are obtained from the dehydrogenation of the micron-sized powder after high-energy ball milling. The high-energy ball milling process is: the ball-to-material ratio is 30:1, the rotation speed is 280rpm, and the ball milling time is 2.5h. The hydrogenation conditions are to maintain the pressure in a hydrogen atmosphere at 275℃ and 2.0MPa for 1.5h, and then to maintain the temperature at 275℃ and 0.01MPa for 20min. The implementation effect of the method of the present invention is as follows Figure 4 As shown in the figure, the particle diameter after hydrogen absorption and desorption is about 19μm, and the internal structure can be clearly seen. The internal structure contains Mg2Ni phase and Mg matrix phase distributed in granular form, which are formed by the decomposition of hydride Mg2NiH4 and MgH2 respectively. After the cycle of hydrogen absorption and desorption, the Mg2Ni phase is evenly distributed on the Mg matrix.

[0066] The specific preparation process includes the following steps:

[0067] 1. Spread the powder 4 to be observed evenly on one end of a copper sheet of 4 mm × 20 mm in size, covering an area of ​​4 mm × 4 mm, and bend the copper sheet 5 mm away from the edge of the area covered by the powder 4 to be observed downward, so that the angle between the bent section of the copper sheet and the test section of the powder to be observed is 91°, presenting an approximately L-shape;

[0068] 2. The powder 4 to be observed is completely coated on the copper sheet with a cold mounting solution 2, wherein the cold mounting solution 2 comprises polymethyl methacrylate CAS9011-14-7 and a metallographic epoxy curing agent, wherein the weight ratio of polymethyl methacrylate CAS9011-14-7 to the metallographic epoxy curing agent is 1:0.9; wherein the main components of the metallographic epoxy curing agent are isophorone diamine, benzoic acid, trimethylcyclohexane dicarboxylic acid and 2,4,6-triphenol;

[0069] 3. After the cold mounting solution 2 fixes the powder 4 to be observed on the conductive metal sheet 1;

[0070] 4. Put the copper sheet into a mold 3 with a cavity inside, fill the cavity inside the mold 3 with the cold mounting solution 2, vertically extend the side of the copper sheet without the observed powder out of the cold mounting solution 2, and the side of the copper sheet with the observed powder 4 faces the bottom of the mold 3, and let it stand at room temperature for 20-30 minutes to solidify;

[0071] 5. After the cold mounting solution 2 solidifies, take out the sample and polish the side containing particles with 800# sandpaper, 1200# sandpaper and 2000# sandpaper respectively until the copper sheet is exposed. Finally, finely polish with 3000# sandpaper and 5000# sandpaper respectively before use for scanning electron microscopy observation. Example

[0072] Preparation of Mg 85 Ni 14.5 In 0.5 The cross section of the alloy particles after high-energy ball milling. The observed particles are obtained after ball milling in a planetary high-energy ball mill. The high-energy ball milling process is: ball-to-material ratio is 30:1, the rotation speed is 280rpm, and the ball milling time is 2.5h. The implementation effect is as follows Figure 5 As shown, the fine Mg-Mg2Ni lamellar eutectic structure inside the alloy can be clearly observed from the particle in the center of the figure, wherein the bright white needle-shaped lamellar layer is the Mg2Ni phase, and the brittle Mg2Ni phase lamellar layer is broken due to the high-speed impact of the stainless steel ball during the ball milling process. The cross section prepared by the method of the present invention can clearly and intuitively show the internal organizational structure of the particle.

[0073] The specific preparation process includes the following steps:

[0074] 1. The powder 4 to be observed after high-energy ball milling is evenly spread on one end of an aluminum sheet of 4mm×20mm in size, covering an area of ​​4mm×4mm. The aluminum sheet 5mm away from the edge of the area covered by the powder 4 to be observed is bent downward, so that the angle between the bent section of the aluminum sheet and the test section of the powder to be observed is 95°, presenting an approximate L-shape;

[0075] 2. The powder to be observed 4 is completely coated on the aluminum sheet with a cold mounting solution 2, wherein the cold mounting solution 2 comprises polymethyl methacrylate CAS9011-14-7 and a metallographic epoxy curing agent, wherein the weight ratio of polymethyl methacrylate CAS9011-14-7 to the metallographic epoxy curing agent is 1:0.8; wherein the main components of the metallographic epoxy curing agent are isophorone diamine, benzoic acid, trimethylcyclohexane dicarboxylic acid and 2,4,6-triphenol;

[0076] 3. After the cold mounting solution 2 fixes the powder 4 to be observed on the conductive metal sheet 1;

[0077] 4. Put the aluminum sheet into a mold 3 with a cavity inside, fill the cavity inside the mold 3 with the cold mounting solution 2, vertically extend the side of the aluminum sheet without the observed powder out of the cold mounting solution 2, and the side of the aluminum sheet with the observed powder 4 faces the bottom of the mold 3, and let it stand at room temperature for 20-30 minutes to solidify;

[0078] 5. After the cold mounting solution 2 solidifies, take out the sample and polish the side containing particles with 800# sandpaper, 1200# sandpaper and 2000# sandpaper respectively until the aluminum sheet is exposed. Finally, finely polish with 3000# sandpaper and 5000# sandpaper respectively before use for scanning electron microscopy observation. Example

[0079] Preparation of semi-hydrogen absorbing Mg 85 Ni 14.6 Ag 0.4 The cross section of the alloy particles is obtained from the powder after high-energy ball milling and hydrogenation. The high-energy ball milling process is: ball-to-material ratio 30:1, rotation speed 270rpm, ball milling time 2.5h. The hydrogenation conditions are 175℃, 0.5MPa hydrogen atmosphere pressure for 0.5h. The implementation effect of the method of the present invention is as follows Figure 6 As shown in the figure, the particle diameters range from a few microns to tens of microns, and the internal structure is clearly visible. In the backscattering mode, since the atomic mass of Ni is larger than that of Mg, the bright white Mg2NiH 0.3 The good structural strength of the embedded material can firmly fix the particles, even the particle cross section smaller than 5μm can be obtained.

[0080] The specific preparation process includes the following steps:

[0081] 1. Evenly spread the incompletely hydrogenated powder 4 to be observed on one end of an aluminum sheet of 4 mm × 20 mm in size, covering an area of ​​4 mm × 4 mm, and bend the aluminum sheet 5 mm away from the edge of the area covered by the powder 4 to be observed downward, so that the angle between the bent section of the aluminum sheet and the test section of the powder to be observed is 93°, presenting an approximately L-shape;

[0082] 2. The powder to be observed 4 is completely coated on the aluminum sheet with a cold mounting solution 2, wherein the cold mounting solution 2 comprises polymethyl methacrylate CAS9011-14-7 and a metallographic epoxy curing agent, wherein the weight ratio of polymethyl methacrylate CAS9011-14-7 to the metallographic epoxy curing agent is 1:0.8; wherein the main components of the metallographic epoxy curing agent are isophorone diamine, benzoic acid, trimethylcyclohexane dicarboxylic acid and 2,4,6-triphenol;

[0083] 3. After the cold mounting solution 2 fixes the powder 4 to be observed on the conductive metal sheet 1;

[0084] 4. Put the aluminum sheet into a mold 3 with a cavity inside, fill the cavity inside the mold 3 with the cold mounting solution 2, vertically extend the side of the aluminum sheet without the observed powder out of the cold mounting solution 2, and the side of the aluminum sheet with the observed powder 4 faces the bottom of the mold 3, and let it stand at room temperature for 20-30 minutes to solidify;

[0085] 5. After the cold mounting solution 2 solidifies, demolding is performed, and the side containing the powder to be observed 4 is polished with 800# sandpaper, 1200# sandpaper and 2000# sandpaper respectively until the aluminum sheet is exposed. Finally, fine polishing is performed with 3000# sandpaper and 5000# sandpaper respectively before use for scanning electron microscopy observation.

[0086] Obviously, the above-mentioned embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the embodiments of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made on the basis of the above description. It is impossible to list all the embodiments here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A method for preparing a micron-sized particle cross section that can be repeatedly used for electron microscope observation, characterized in that: The steps include: Step 1: comprising a conductive metal sheet (1), wherein the conductive metal sheet (1) comprises a powder test section to be observed and a bending section, and spreading the powder to be observed (4) on one side of the powder test section to be observed of the conductive metal sheet (1); Step 2: using a cold mounting solution (2) to fill the spaces and cracks between the powders to be observed (4) and completely cover the conductive metal sheet (1), wherein the cold mounting solution (2) comprises polymethyl methacrylate CAS9011-14-7 and a metallographic epoxy curing agent; Step 3: The powder to be observed (4) is fixed on the conductive metal sheet (1) by using a cold mounting solution (2); Step 4: placing the conductive metal sheet (1) in step 3 into a mold (3) having a cavity therein, filling the cavity in the mold (3) with a cold embedding solution (2), extending one end of the bent section of the conductive metal sheet (1) vertically out of the cold embedding solution (2), and arranging the side of the powder test section to be observed provided with the powder to be observed (4) toward the bottom of the mold (3); the angle between the bent section and the powder test section to be observed is greater than or equal to 85° and less than 90° or greater than 90° and less than or equal to 95°; the powder test section to be observed is covered with the powder to be observed (4), and the distance between the edge of the area covered by the powder to be observed (4) and the bent section is 5-8 mm; Step 5: After the cold mounting solution (2) filled in the mold in step 4 is solidified, demolding is performed, and then the covered area containing the powder to be observed (4) is polished to obtain a particle cross section for scanning electron microscopy observation.

2. The method for preparing a micron-sized particle cross section that can be repeatedly used for electron microscope observation according to claim 1, characterized in that: The conductive metal sheet (1) is a copper sheet or an aluminum sheet with a thickness of 0.2 mm to 0.5 mm.

3. The method for preparing a micron-sized particle cross section that can be repeatedly used for electron microscope observation according to claim 1, characterized in that: The mold (3) is a square or cylindrical silicone soft mold.

4. The method for preparing micron-sized particle cross sections that can be repeatedly used for electron microscope observation according to claim 1, characterized in that: The weight ratio of the polymethyl methacrylate CAS9011-14-7 to the metallographic epoxy curing agent is 1:(0.7-0.9).

5. The method for preparing micron-sized particle cross sections that can be repeatedly used for electron microscope observation according to claim 1, characterized in that: The polishing in step 5 includes: Step A: grinding the demoulded conductive metal sheet (1) with 800# sandpaper, 1200# sandpaper and 2000# sandpaper respectively until the powder to be observed (4) is exposed; Step B: Finely grind the powder (4) to be observed in step A with 3000# sandpaper and 5000# sandpaper respectively to obtain the particle cross section of the powder (4) to be observed.

Citation Information

Patent Citations

  • Preparation method of magnetic powder particle transmission electron microscope sample

    CN112786270A

  • Method for embedding radioactive sample in hot chamber for improving conductivity and embedded sample

    CN114199917A