A preparation method of lithium ion sieve H2TiO3 adsorption curtain membrane and a salt lake lithium extraction system using the curtain membrane
By preparing a lithium-ion sieve H2TiO3 adsorption curtain membrane, the problems of lithium-ion sieve powder loss and cumbersome existing membrane preparation processes have been solved, realizing the reuse of lithium-ion sieves and efficient adsorption for lithium extraction from salt lakes, which has industrialization potential.
Patent Information
- Application Number
- CN202211392919.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-11-08
AI Technical Summary
The direct use of existing lithium-ion sieve powder leads to loss, making it difficult to achieve industrial application. Furthermore, the existing membrane preparation process is cumbersome and cannot be industrialized on a large scale.
A lithium-ion sieve H2TiO3 adsorption curtain membrane was prepared by blending H2TiO3 with PVDF binder, spinning it into hollow fiber membrane filaments, and then making it into a curtain membrane module for lithium extraction from salt lakes.
This technology enables the reuse of lithium-ion sieves, reduces costs, and improves the adsorption rate of lithium extraction from salt lakes, showing broad application prospects.
Smart Images

Figure BDA0003932766010000061 
Figure BDA0003932766010000071 
Figure BDA0003932766010000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium extraction from salt lakes, in particular to a method for preparing a lithium ion sieve H2TiO3 adsorption curtain membrane that can be used to intercept lithium ions in water, and also relates to a salt lake lithium extraction system using the lithium ion sieve H2TiO3 adsorption curtain membrane obtained by the preparation method. Background Art
[0002] Lithium is the lightest metal element. As the application of lithium in the field of new energy materials becomes increasingly apparent, the mining of lithium resources has attracted widespread attention. my country has abundant reserves of lithium resources, and the lithium reserves in salt lake brine are as high as 70%. Therefore, the comprehensive development and utilization of salt lake brine lithium resources has become the main development direction of the lithium industry. Using lithium ion sieves for adsorption and lithium extraction is a green method with application prospects. It is not only simple in process, but also has a high adsorption capacity. It is one of the most industrially potential lithium extraction methods. At present, most of the lithium ion sieve adsorbents on the market are nano-scale powders. Direct use will cause powder loss, which is not easy to operate industrially, hindering its commercial application. Therefore, many scholars granulate, make films or load lithium ion sieves into nanofibers to achieve better application effects.
[0003] Patent CN108358278A discloses a method for extracting lithium from salt lake brine using a hollow fiber forward osmosis membrane. First, a conventional method is used to prepare a hollow fiber base membrane by phase inversion. Then, the base membrane is soaked in a solution such as sodium hydroxide to form an electrostatic activation layer on the surface of the base membrane. Subsequently, the hollow fiber forward osmosis membrane is obtained by self-assembly layer by layer through multiple cycles of soaking in different cationic electrolyte solutions. The membrane prepared by this method has a complicated operation process and needs to be soaked in cationic electrolyte solutions repeatedly. At the same time, the membrane obtained by this method cannot achieve large-scale industrial lithium extraction.
[0004] Patent CN104906966A discloses a hollow fiber forward osmosis membrane. In the patent, graphene is added to a solvent composed of N-methylpyrrolidone or dimethylacetamide or dimethylformamide and 1,4-dioxane, and polyethylene glycol or polyvinylpyrrolidone / lithium chloride composite additives are added. After stirring, cellulose acetate is added to obtain a casting solution, and finally the solution is solidified to obtain a forward osmosis membrane. However, the patent only describes the preparation method of the membrane, and does not involve whether the membrane is suitable for use in lithium extraction from salt lake brine. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a H2TiO3 lithium ion sieve, which is then blended with a PVDF binder, spun into hollow fiber membrane yarns and then made into a curtain-type membrane module, which is used to extract lithium from salt lakes, thereby overcoming the loss problem caused by direct use of lithium ion sieve powder, and expecting to reduce costs and achieve partial material recycling.
[0006] Based on this, the present invention provides a method for preparing a lithium ion sieve H2TiO3 adsorption curtain membrane, the method comprising the following steps:
[0007] (1) Preparation of lithium ion sieve precursor Li2TiO3
[0008] 0.1-0.5 mol of butyl titanate and 0.2-1 mol of lithium nitrate are placed in anhydrous ethanol, and stirred thoroughly to obtain a suspension, and the obtained suspension is subjected to ultrasonic treatment to obtain a uniform mixture, and the obtained mixture is dried and calcined at a temperature of 700-1000° C. for 3-5 hours, and cooled to obtain a lithium ion sieve precursor Li2TiO3;
[0009] (2) Preparation of lithium ion sieve H2TiO3
[0010] The lithium ion sieve precursor Li2TiO3 obtained in step (1) is placed in 0.2-0.5 mol / L hydrochloric acid to make the molar ratio of micro-Li2TiO3 to HCl be 1:3-1:5, and the slurry is filtered after being fully stirred. The obtained solid phase is thoroughly washed with deionized water, and the solid phase is dried and ground to obtain a white powder, which is the lithium ion sieve micro-H2TiO3;
[0011] (3) Preparation of casting solution
[0012] Prepare H2TiO3 / PVDF spinning solution: weigh 1-5kg of polyvinylidene fluoride, add it to 3-15kg of N,N-dimethylacetamide, and stir it thoroughly at 60-70°C until the polyvinylidene fluoride is completely dissolved; then add 1-5kg of polyvinyl pyrrolidone and 1-2kg of polyethylene glycol PEG-400, continue stirring until dissolved, and obtain a mixed solvent; weigh 1-5kg of the lithium ion sieve powder obtained in step (2), sieve it, and slowly add it to the mixed solution, stir it thoroughly until the materials are evenly mixed, and obtain H2TiO3 / PVDF casting solution;
[0013] (4) Preparation of curtain membrane module composed of hollow fiber membrane
[0014] After the casting liquid in step (3) is degassed, the casting liquid is extruded into a coagulation bath at 50-70°C through a wet spinning device, and solidified H2TiO3 / PVDF hollow fibers are obtained after standing. The obtained hollow fibers are rolled up and, after cutting, alignment, fixing, and sealing, a lithium ion sieve H2TiO3 adsorption curtain membrane is obtained.
[0015] According to a preferred embodiment, the ultrasonic treatment time in step (1) is 30-60 min.
[0016] In the present invention, the content of lithium ions in the H2TiO3 / PVDF casting solution in step (2) is 10%-30% by total weight.
[0017] Preferably, the screening in step (3) is through a 100-150 mesh sieve.
[0018] In the present invention, the coagulation bath in step (4) is a DMAC aqueous solution containing 10% to 20% by weight.
[0019] The present invention also provides a salt lake lithium extraction system using a lithium ion sieve H2TiO3 adsorption curtain membrane, the system comprising a tank body (1), a hydrochloric acid storage tank (2), a salt lake brine storage tank (3) and a hollow fiber curtain membrane assembly (4), wherein the hydrochloric acid storage tank (2) and the salt lake brine storage tank (3) are respectively connected to the bottom of the tank body (1) through pipelines, wherein the hollow fiber curtain membrane assembly (4) is a hollow fiber curtain membrane assembly obtained according to the aforementioned preparation method, and the hydrochloric acid storage tank (2) is filled with 0.05-0.3 mol / L dilute hydrochloric acid as an eluent.
[0020] The system operates as follows:
[0021] (1) Adsorption stage
[0022] Adsorption begins: lithium-containing salt lake brine enters the pool body (1) from the salt lake brine storage tank (3), with a hydraulic retention time of 0.5-3 BV / h. When the water level of the pool body (1) reaches 80%-90% of the pool height, the hollow fiber ultrafiltration membrane (4) is negatively pressured by a negative pressure suction device to obtain produced water;
[0023] Stop adsorption: monitor the lithium ion concentration in the produced water. When the lithium ion concentration in the produced water is the same as the lithium ion concentration in the salt lake brine storage tank (3), it is considered that the adsorption of the curtain membrane module has reached saturation. At this time, the salt lake brine storage tank (3) stops feeding water into the pool body (1), and the remaining salt lake brine in the pool body (1) is discharged;
[0024] (2) Elution stage
[0025] The dilute hydrochloric acid tank of the hydrochloric acid storage tank (2) is introduced into the pool body (1), and the negative pressure suction device of the curtain membrane module is started so that the hydraulic retention time of the dilute hydrochloric acid on the membrane module is 1BV / h. The pH value of the membrane produced water is monitored. When the pH value is the same as the pH value of the dilute hydrochloric acid in the hydrochloric acid storage tank (3), the introduction of the eluent is stopped and the dilute hydrochloric acid in the pool body (1) is transported back to the hydrochloric acid storage tank (2). At this time, the elution stage is ended and the adsorption stage is re-entered.
[0026] According to a preferred embodiment, the mechanical stirring time of step (1) is 1-2 hours, until the materials are fully mixed.
[0027] In the present invention, the ratio of polyvinyl chloride, polyvinyl butyral and polyvinylidene fluoride in step (2) is 1:1-2:1-3.
[0028] Preferably, in step (2), polyvinyl chloride, polyvinyl butyral, polyvinylidene fluoride, nanoscale lithium ion sieve precursor Li2TiO3 and dimethylacetamide are stirred at 50-80°C for 5-10 hours to obtain a mixed slurry. Deionized water is added to the mixed slurry at a flow rate of 0.1-1 L / min.
[0029] The present invention verifies through experiments that the salt lake lithium extraction system using the lithium ion sieve H2TiO3 adsorption curtain membrane can effectively extract lithium ions from brine without adsorbing other ions in the brine. The curtain membrane is eluted with an acid solution to achieve the recycling of the lithium ion sieve curtain membrane.
[0030] In addition, compared with the prior art, the adsorption rate of lithium extraction from salt lakes using the lithium ion sieve H2TiO3 adsorption curtain membrane of the present invention is greatly improved, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is a SEM photograph of the lithium ion sieve H2TiO3 of Example 1;
[0032] Figure 2 is a SEM photograph of the hollow fiber membrane of Example 1;
[0033] Figure 3 is the adsorption efficiency of the hollow fiber membrane module of Example 1;
[0034] Figure 4 is a schematic structural diagram of the salt lake lithium extraction system of Example 1;
[0035] Among them, 1. Pool body; 2. Hydrochloric acid storage tank; 3. Salt lake brine storage tank; 4. Membrane module; 5. Pump;
[0036] Figure 5 is a SEM photograph of the lithium ion sieve H2TiO3 of Example 2;
[0037] Figure 6 is a SEM photograph of the hollow fiber membrane of Example 2;
[0038] Figure 7 is the adsorption efficiency of the hollow fiber membrane module of Example 2. DETAILED DESCRIPTION
[0039] The following examples are used to explain the technical solutions of the present invention in a non-limiting manner.
[0040] In the present invention, unless otherwise specified, "%" used to describe concentration refers to mass percentage, and ":" refers to mass ratio.
[0041] Example 1
[0042] Preparation of lithium adsorbent precursor Li2TiO3: 0.1 mol of butyl titanate and 0.2 mol of lithium nitrate are mixed in anhydrous ethanol, stirred for 3 hours under the action of magnetic stirring, and then the suspension is treated with ultrasound for 30 minutes to obtain a uniform mixture; the mixture is further dried at 50°C, and then placed in a tubular furnace and calcined at 700°C for 3 hours. After cooling to room temperature, Li2TiO3 white powder is obtained, i.e., the lithium adsorbent precursor Li2TiO3.
[0043] Preparation of lithium adsorbent H2TiO3: Place Li2TiO3 in a 0.2 mol / L dilute HCl solution, stir it at a constant temperature for 4 hours in a 60°C water bath, filter it, wash it 3 times with deionized water, dry it and grind it to obtain white H2TiO3 powder. Figure 1 This is a scanning electron microscope image of dry H2TiO3 powder.
[0044] Preparation of H2TiO3 / PVDF spinning solution: 1 kg of recycled polyvinylidene fluoride (PVDF) was added to 3 kg of N,N-dimethylacetamide (DMAC) organic solvent, heated to 60°C at a constant temperature, and mechanically stirred to fully dissolve the polyvinylidene fluoride (PVDF); then 1 kg of polyvinyl pyrrolidone (PVP-K30) and polyethylene glycol (PEG-400) were added, and heating and stirring were continued until dissolved; finally, after it was completely dissolved, 1 kg of the above-mentioned dry H2TiO3 powder passed through a 150-mesh sieve was slowly added to the polyvinylidene fluoride (PVDF) organic solution, and mechanically stirred for 1 hour to fully mix the feed liquid to obtain H2TiO3 / PVDF casting solution.
[0045] Preparation of H2TiO3 / PVDF hollow fiber membrane: First, the obtained feed liquid is degassed, and then the spinning solution is injected into the wet spinning equipment (TS-01-20 of Lingxian Textile Equipment Co., Ltd., China), the membrane rope is fixed at the spinneret, and the membrane rope is pulled by the roller. The spinning machine extrude the spinning solution through the spinneret, and the spinning solution wraps the membrane rope and then enters the coagulation bath at 50°C, and the mass exchange occurs through the water phase to obtain H2TiO3 / PVDF hollow fiber. The solidified fiber is collected on the automatic winding roller for standby use. Figure 2 Surface and cross-sectional images of H2TiO3 / PVDF hollow fibers.
[0046] Preparation of H2TiO3 / PVDF curtain membrane module: First, the H2TiO3 / PVDF hollow fiber is cut into membrane filaments of uniform length, and 50 membrane filaments are arranged in a group. The pore-plugging agent is applied on both ends of the membrane filament group, and then the two ends of the membrane filament group are sealed with glue. After the sealing glue is completely cured, the ends are fixed in the card slot of the curtain membrane module to obtain a lithium-adsorbed H2TiO3 / PVDF module.
[0047] Build as Figure 4 The system shown includes a volume of 5m 3 A pool body 1, a hydrochloric acid storage tank 2, a salt lake brine storage tank 3 and a hollow fiber curtain membrane module 4. The hydrochloric acid storage tank 2 and the salt lake brine storage tank 3 are respectively connected to the bottom of the pool body 1 through pipelines. The hollow fiber curtain membrane module 4 produces water through a pump, and an online lithium concentration detection and a pH online detection are set on the water production pipeline.
[0048] Adsorption process: 10 lithium adsorption H2TiO3 / PVDF devices are placed in the pool body 1, and a pump is installed on the upper part of the device. When the salt lake brine in the pool body 1 is pumped out, the water passes through the lithium adsorption H2TiO3 / PVDF device. During the adsorption process, the salt lake brine flows through the lithium adsorption H2TiO3 / PVDF device at a flow rate of 1BV / h to extract lithium ions. The lithium ion sieve H2TiO3 adsorbs the lithium ions in the brine and extracts the lithium ions in the brine. When the lithium ion concentration at the water outlet is consistent with the concentration before the water inlet, it means that the lithium adsorption H2TiO3 / PVDF device has reached saturated adsorption. After saturated adsorption, the pump at the bottom of the water tank is used to discharge the salt lake brine from the drain below back to the salt lake brine bucket, and then eluted with an acid solution.
[0049] Elution process: Select 0.2mol / L HCl solution as the eluent, and elute at a flow rate of 1BV / h. When the HCl solution passes through the saturated lithium adsorption H2TiO3 / PVDF assembly, the hydrogen ions in the HCl solution elute the lithium in the lithium ion sieve. Add a pH test detector at the water outlet. When the pH value of the solution at the water outlet is consistent with that before the water inlet, it means that the HCl solution has completely eluted the lithium ions in the lithium adsorption H2TiO3 / PVDF assembly. This process realizes the elution of the lithium adsorption H2TiO3 / PVDF assembly. After the elution is complete, use the water pump at the bottom of the water tank to discharge the HCl solution from the drain below into the HCl solution barrel, and then open the salt lake brine inlet valve to start a new round of salt lake brine lithium extraction process.
[0050] The concentrations of various ions in the influent and produced water during the lithium extraction and elution process are shown in Table 1. From Table 1, it can be seen that the lithium ions in the brine can be effectively extracted by using the lithium adsorption H2TiO3 / PVDF assembly as a lithium extraction device. The lithium ion concentration in the salt lake brine is 260 mg / L, and the lithium ion concentration of the produced water after lithium extraction is 25.8 mg / L, indicating that the assembly can extract lithium ions in the brine. Figure 7A comparison chart of the adsorption efficiency of lithium ion adsorbents and lithium adsorbent H2TiO3 / PVDF devices sold on the market shows that the adsorption rate of current lithium adsorbents is very slow, requiring about 3 hours, while the lithium adsorbent H2TiO3 / PVDF device only takes about 1.2 hours, greatly improving the adsorption rate.
[0051] Table 1 Lithium adsorption on H2TiO 3 / Results of lithium extraction process of PVDF module
[0052]
[0053]
[0054] Example 2
[0055] Preparation of lithium adsorbent precursor Li2TiO3: 0.5 mol of butyl titanate and 1 mol of lithium nitrate are mixed in anhydrous ethanol, stirred for 5 hours under the action of magnetic stirring, and then the suspension is treated with ultrasound for 60 minutes to obtain a uniform mixture; the mixture is further dried at 60°C, and then placed in a tubular furnace and calcined at 1000°C for 5 hours. After cooling to room temperature, Li2TiO3 white powder is obtained, i.e., the lithium adsorbent precursor Li2TiO3.
[0056] Preparation of lithium adsorbent H2TiO3: Place Li2TiO3 in a 0.5 mol / L dilute HCl solution, stir it at a constant temperature for 5 hours in a 70°C water bath, filter it, wash it with deionized water 5 times, dry it and grind it to obtain white H2TiO3 powder. Figure 5 This is a scanning electron microscope image of dry H2TiO3 powder.
[0057] Preparation of H2TiO3 / PVDF spinning solution: 5kg of recycled polyvinylidene fluoride (PVDF) was added to 15kg of N,N-dimethylacetamide (DMAC) organic solvent, heated to 70°C at a constant temperature, and mechanically stirred to fully dissolve the polyvinylidene fluoride (PVDF); then 5kg of polyvinyl pyrrolidone (PVP-K30) and polyethylene glycol (PEG-400) were added, and heating and stirring were continued until dissolved; finally, after it was completely dissolved, 5kg of the above-mentioned dry H2TiO3 powder passed through a 150-mesh sieve was slowly added to the polyvinylidene fluoride (PVDF) organic solution, and mechanically stirred for 1h to fully mix the feed liquid to obtain H2TiO3 / PVDF casting solution.
[0058] Preparation of H2TiO3 / PVDF hollow fiber membrane: First, the obtained feed liquid is degassed, and then the spinning solution is injected into the wet spinning equipment (TS-01-20 of Lingxian Textile Equipment Co., Ltd., China), the membrane rope is fixed at the spinneret, and the membrane rope is pulled by the roller. The spinning machine extrude the spinning solution through the spinneret, and the spinning solution wraps the membrane rope and then enters the coagulation bath at 70°C, and the mass exchange occurs through the water phase to obtain H2TiO3 / PVDF hollow fiber. The solidified fiber is collected on the automatic winding roller for standby use. Figure 6 Surface and cross-sectional images of H2TiO3 / PVDF hollow fibers.
[0059] Preparation of H2TiO3 / PVDF curtain membrane module: First, the H2TiO3 / PVDF hollow fiber is cut into membrane filaments of uniform length. 100 membrane filaments are arranged in a group and pore plugging agent is applied on both ends. Then, the two ends of the membrane filament group are sealed with glue. After the sealing glue is completely cured, the ends are fixed in the card slot of the curtain membrane module to obtain a lithium adsorbed H2TiO3 / PVDF module.
[0060] Similar to Example 1, adsorption process: at 10 m 3 20 lithium adsorption H2TiO3 / PVDF devices are placed in the pool body, and a pump is installed on the upper part of the device to extract the salt lake brine in the pool body, so that the water body passes through the lithium adsorption H2TiO3 / PVDF device. During the adsorption process, the salt lake brine flows through the lithium adsorption H2TiO3 / PVDF device at a flow rate of 5BV / h to extract lithium ions. The lithium ion sieve H2TiO3 adsorbs the lithium ions in the brine and extracts the lithium ions in the brine. When the lithium ion concentration at the water outlet is consistent with the concentration before the water inlet, it means that the lithium adsorption H2TiO3 / PVDF device has reached saturated adsorption. After saturated adsorption, the pump at the bottom of the water tank is used to discharge the salt lake brine from the drain below back to the salt lake brine bucket, and then it is eluted with an acid solution.
[0061] Elution process: Select 0.5mol / L HCl solution as the eluent, and elute at a flow rate of 5BV / h. When the HCl solution passes through the saturated lithium adsorption H2TiO3 / PVDF assembly, the hydrogen ions in the HCl solution elute the lithium in the lithium ion sieve. Add a pH test detector at the water outlet. When the pH value of the solution at the water outlet is consistent with that before the water inlet, it means that the HCl solution has completely eluted the lithium ions in the lithium adsorption H2TiO3 / PVDF assembly. This process realizes the elution of the lithium adsorption H2TiO3 / PVDF assembly. After the elution is complete, use the water pump at the bottom of the water tank to discharge the HCl solution from the drain below into the HCl solution barrel, and then open the salt lake brine inlet valve to start a new round of salt lake brine lithium extraction process.
[0062] The concentrations of various ions in the influent and produced water during the lithium extraction and elution process are shown in Table 2. From Table 2, it can be seen that the lithium ions in the brine can be effectively extracted by using the lithium adsorption H2TiO3 / PVDF assembly as a lithium extraction device. The lithium ion concentration in the salt lake brine is 260 mg / L, and the lithium ion concentration of the produced water after lithium extraction is 16.7 mg / L, indicating that the assembly can extract lithium ions in the brine.
[0063] Figure 7 A comparison chart of the adsorption efficiency of lithium ion adsorbents and lithium adsorbent H2TiO3 / PVDF devices sold on the market shows that the adsorption rate of the current lithium adsorbent is very slow, requiring 3 hours, while the lithium adsorbent H2TiO3 / PVDF device only takes 0.5 hours, greatly improving the adsorption rate.
[0064] Table 2 Results of lithium extraction process of lithium adsorption H2TiO3 / PVDF assembly
[0065]
Claims
1. A salt lake lithium extraction system using a lithium ion sieve H2TiO3 adsorption curtain membrane, the system comprising a cell body (1), a hydrochloric acid storage tank (2), a salt lake brine storage tank (3) and a hollow fiber curtain membrane module (4), wherein the hydrochloric acid storage tank (2) and the salt lake brine storage tank (3) are respectively connected to the bottom of the cell body (1) through pipelines, characterized in that The hydrochloric acid storage tank (2) contains 0.05-0.3 mol / L dilute hydrochloric acid as an eluent. The hollow fiber curtain membrane assembly (4) is a lithium ion sieve H2TiO3 adsorption curtain membrane. The preparation method of the curtain membrane comprises the following steps: (1) Preparation of lithium ion sieve precursor Li2TiO3 0.1-0.5 mol of butyl titanate and 0.2-1 mol of lithium nitrate are placed in anhydrous ethanol, and the mixture is stirred thoroughly to obtain a suspension, and the suspension is subjected to ultrasonic treatment to obtain a uniform mixture, and the mixture is dried and calcined at a temperature of 700-1000° C. for 3-5 hours, and the lithium ion sieve precursor Li2TiO3 is obtained after cooling; (2) Preparation of lithium ion sieve H2TiO3 The lithium ion sieve precursor Li2TiO3 obtained in step (1) is placed in 0.2-0.5 mol / L hydrochloric acid to make the molar ratio of Li2TiO3 to HCl be 1:3-1:5, and the slurry is filtered after being fully stirred. The obtained solid phase is thoroughly washed with deionized water, and the solid phase is dried and ground to obtain a white powder, which is the lithium ion sieve H2TiO3; (3) Preparation of casting solution Preparation of H2TiO3 / PVDF spinning solution: weigh 1-5 kg of polyvinylidene fluoride, add it to 3-15 kg of N,N-dimethylacetamide, and stir it thoroughly at 60-70°C until the polyvinylidene fluoride is completely dissolved; then add 1-5 kg of polyvinyl pyrrolidone and 1-2 kg of polyethylene glycol PEG-400, continue stirring until dissolved, and obtain a mixed solution; weigh 1-5 kg of the lithium ion sieve powder obtained in step (2), sieve it and slowly add it to the mixed solution, stir it thoroughly until the materials are evenly mixed, and obtain H2TiO3 / PVDF casting solution; the content of the lithium ion sieve in step (3) in the H2TiO3 / PVDF casting solution is 10%-30% by total weight; (4) Preparation of lithium ion sieve H2TiO3 adsorption curtain membrane After the casting liquid in step (3) is degassed, the casting liquid is extruded into a coagulation bath at 50-70°C by a wet spinning device, and H2TiO3 / PVDF hollow fibers are obtained after coagulation. The obtained hollow fibers are rolled up, and after cutting, alignment, fixing, and plugging, a lithium ion sieve H2TiO3 adsorption curtain membrane is obtained.
2. The salt lake lithium extraction system according to claim 1, characterized in that The ultrasonic treatment time of step (1) is 30-60 min.
3. The salt lake lithium extraction system according to claim 1, characterized in that The sieving in step (3) is through a 100-150 mesh sieve.
4. The salt lake lithium extraction system according to claim 1, characterized in that The coagulation bath in step (4) is a 10% to 20% by weight DMAC aqueous solution.
5. The salt lake lithium extraction system according to claim 1, characterized in that The system operates as follows: (1) Adsorption stage Adsorption begins: lithium-containing salt lake brine enters the pool body (1) from the salt lake brine storage tank (3), and the hydraulic retention time is 0.5-3BV / h. When the water level of the pool body (1) reaches 80%-90% of the pool height, the hollow fiber curtain membrane module (4) is negatively pressured and sucked by a negative pressure suction device to obtain produced water; Stop adsorption: monitor the lithium ion concentration in the produced water. When the lithium ion concentration in the produced water is the same as the lithium ion concentration in the salt lake brine storage tank (3), it is considered that the adsorption of the curtain membrane module has reached saturation. At this time, the salt lake brine storage tank (3) stops feeding water into the pool body (1), and the remaining salt lake brine in the pool body (1) is discharged; (2) Elution stage The dilute hydrochloric acid tank of the hydrochloric acid storage tank (2) is introduced into the pool body (1), and the negative pressure suction device of the curtain membrane module is started so that the hydraulic retention time of the dilute hydrochloric acid on the membrane module is 1 BV / h. The pH value of the membrane produced water is monitored. When the pH value is the same as the pH value of the dilute hydrochloric acid in the hydrochloric acid storage tank (2), the introduction of the eluent is stopped and the dilute hydrochloric acid in the pool body (1) is transported back to the hydrochloric acid storage tank (2). At this time, the elution stage is ended and the adsorption stage is re-entered.