Maleic acid monocorn starch ester modified nitrile rubber adhesive and preparation method thereof
Through the cross-linking technology of cornstarch maleate-modified nitrile rubber adhesive, the problems of insufficient bonding force, mechanical strength and water resistance of existing nitrile rubber adhesives are solved, and high adhesion is achieved. Improved strength, mechanical strength and fire resistance, suitable for many industrial fields.
Patent Information
- Application Number
- CN202110938959.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-16
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-08-16
AI Technical Summary
Existing nitrile rubber adhesives have problems such as low initial adhesion, weak mechanical strength, and poor fire resistance and water resistance.
Using corn starch maleate modified nitrile rubber adhesive, cross-linking maleic anhydride esterified corn starch and nitrile rubber, adding zinc oxide, sulfur, carbon black, petroleum resin, antioxidant and coupling agent, prepared through mechanical blending and cross-linking, forming a dual network structure to improve adhesion and water resistance.
It significantly improves the adhesive force, mechanical strength, water resistance and fire resistance of the adhesive, simplifies the preparation process, has low cost and is suitable for electronic industry, aerospace and other fields.
Smart Images

Figure 529446DEST_PATH_IMAGE002 
Figure 587532DEST_PATH_IMAGE004
Abstract
Description
Technical Field
[0001] The invention relates to adhesive field technology, in particular to a maleic acid monocorn starch ester modified nitrile rubber adhesive and a preparation method thereof. Background Art
[0002] With the continuous development of science and technology and the continuous improvement of people's living standards, adhesives with traditional molecular structures (such as inorganic adhesives) are now insufficient to meet people's applications in production and life, and polymer materials have become an important research direction for adhesives. Adhesives composed of polymer compounds can generally be divided into two categories: natural adhesives and synthetic adhesives. Natural adhesives refer to adhesive substances that can be extracted from natural animals and plants and can be directly used. Most synthetic adhesives are composed of synthetic polymers, such as synthetic resins, synthetic rubber adhesives and special adhesives. Compared with the restrictive application of natural adhesives, synthetic adhesives are increasingly used in aerospace, automobiles, machinery and electronics. Among them, nitrile rubber adhesives have been widely used in machinery, automobiles, construction, aviation, shipbuilding industry and military industry due to their good aging resistance, air tightness and excellent bonding properties. Nitrile rubber adhesives are made of nitrile rubber as the main body and other component raw materials. During the aging process, nitrile rubber adhesives will not produce volatile substances that are harmful to metals, plastics and fabrics due to degradation like chloroprene rubber adhesives. However, currently commercial nitrile rubber adhesives generally have hidden dangers such as low initial adhesion, weak mechanical strength, poor fire resistance and water resistance. Therefore, it is necessary to modify nitrile rubber to obtain an ideal adhesive system. Summary of the invention
[0003] In view of this, the present invention aims at the deficiencies in the prior art, and its main purpose is to provide a maleic acid monocorn starch ester modified nitrile rubber adhesive and a preparation method thereof, which has the characteristics of strong adhesion, high mechanical strength, good fire resistance, excellent water resistance, simple preparation process and easy use.
[0004] To achieve the above purpose, the present invention adopts the following technical solutions:
[0005] A maleic acid monocorn starch ester modified nitrile rubber adhesive. The raw materials for preparing the maleic acid monocorn starch ester modified nitrile rubber adhesive include, by weight: 15-40 parts of corn starch, 30-60 parts of sodium hydroxide solution, 120-300 parts of anhydrous ethanol, 350-500 parts of acetone, 150-350 parts of methyl isobutyl ketone, 20-40 parts of maleic anhydride, 80-100 parts of nitrile rubber, 0.5-2 parts of zinc oxide, 0.5-2 parts of sulfur, 1-2 parts of carbon black, 1-4 parts of petroleum resin, 0.1-1 parts of antioxidant and 0.1-1 parts of coupling agent.
[0006] Preferably, the corn starch is 20, 25 or 30 parts, sodium hydroxide solution is 50 parts, anhydrous ethanol is 200 parts, acetone is 400 parts, methyl isobutyl ketone is 200 parts, maleic anhydride is 27.5 parts, nitrile rubber is 100 parts, zinc oxide is 1 part, petroleum resin is 3 parts, sulfur is 1 part, carbon black is 1.5 parts, antioxidant is 0.5 parts and coupling agent is 0.5 parts.
[0007] Preferably, the mass fraction of the sodium hydroxide solution is 20%.
[0008] Preferably, the antioxidant is hydroquinone, dimethyl hydroquinone or propyl gallate, and preferentially, the antioxidant is hydroquinone.
[0009] Preferably, the coupling agent is a silane coupling agent.
[0010] Preferably, the solvent is one or more of anhydrous ethanol, acetone, butanone, methyl ethyl ketone, ethyl acetate, acetic acid, ethyl ester and methyl isobutyl ketone.
[0011] A method for preparing a maleic acid monocorn starch ester modified nitrile rubber adhesive comprises the following steps:
[0012] (1) Add corn starch, sodium hydroxide solution and anhydrous ethanol into a 100 mL three-necked flask at room temperature and reflux for 1.5-3 h. After cooling, wash with acetone solution and then filter. Then, place the sample in a 50 °C drying oven and dry for 2-5 h to obtain activated corn starch.
[0013] (2) Pour the activated corn starch obtained in step (1) into a 100 mL three-necked flask, then slowly pour the acetone solution into the three-necked flask, stir magnetically at room temperature for 10-20 min, then heat and stir at 40-70 °C for 20-40 min;
[0014] (3) Add maleic anhydride to the acetone solution and stir until the maleic anhydride is completely dissolved; then slowly dropwise add the obtained maleic anhydride acetone solution to the three-necked flask in step (2); after the dropwise addition is completed, react at a constant temperature of 40-70°C for 4-6 hours; after the reaction is completed, cool the mixed solution, wash it with an acetone solution, and then filter it; place the filtered sample in a drying oven at 40-60°C and dry it to constant weight, thereby obtaining monocorn starch maleate;
[0015] (4) setting the roller distance of the nitrile rubber to 2-3 mm on an open mill for plasticizing for 1-5 min, then sequentially adding zinc oxide, carbon black, sulfur, petroleum resin, antioxidant and coupling agent for mixing, setting the roller distance to 0.5-2 mm, and after mixing evenly, adjusting the roller distance to sheet the nitrile rubber;
[0016] (5) using a shredder to shred the nitrile rubber sheet in step (4), pouring the shredded nitrile rubber sheet into a methyl isobutyl ketone solution, and mechanically stirring to dissolve the nitrile rubber sheet to obtain a uniform slurry, the mechanical stirring speed being 800-1000 r / min;
[0017] (6) slowly adding the monocorn starch maleate obtained in step (3) to the nitrile rubber mortar in step (5) under mechanical stirring at a speed of 800-1000 r / min for a stirring time of 30-50 min to obtain an adhesive mortar;
[0018] (7) The adhesive slurry prepared in step (6) is poured into a polytetrafluoroethylene mold and dried at 120° C. for 24 h to form an adhesive film, thereby obtaining a maleic acid monocorn starch ester-modified nitrile rubber adhesive.
[0019] Compared with the prior art, the present invention has obvious advantages and beneficial effects. Specifically, it can be seen from the above technical solution that:
[0020] The preparation method of the maleic acid monocorn starch ester modified nitrile adhesive provided by the present invention uses maleic anhydride as an esterifying agent, corn starch and nitrile rubber as raw materials, and adds the adhesive matching components: zinc oxide, sulfur, carbon black, petroleum resin, antioxidant, and coupling agent through mechanical blending and cross-linking in different proportions. In the above formula, maleic acid monocorn starch ester is first prepared by esterifying corn starch with maleic anhydride, and other adhesive matching components are screened to prepare maleic acid monocorn starch ester modified nitrile adhesive. The adhesive benefits from the individuality and complementary properties of maleic acid monocorn starch ester and nitrile rubber. Maleic anhydride belongs to the starch ester of dicarboxylic acid, which converts the hydroxyl groups on the corn starch molecular chain into ester groups, and can improve the interfacial compatibility of corn starch and nitrile rubber. Compared with the weak comprehensive properties of ordinary corn starch modified nitrile rubber such as initial viscosity, drying and water resistance, maleic acid monocorn starch ester has a large number of polar groups and reactive groups in its macromolecular structure, such as hydroxyl, carboxyl, carbon-carbon double bond, and ester group. The strong polarity and high activity of these groups are favorable factors for promoting the infiltration, diffusion, and adhesion of maleic acid monocorn starch ester to materials, that is, the formation of physical bonding and chemical bonding. Hydroxyl and carboxyl groups can react with metal oxides to form complexes, and can form strong chemical bonding with metal surfaces; at the same time, hydroxyl and carboxyl groups can also react with cyanide groups in nitrile rubber molecules, so that the maleic acid monocorn starch ester network and the nitrile rubber network form a whole, forming a double network structure. Thereby, the reinforcing effect of maleic acid monocorn starch ester on nitrile rubber is greatly improved. Therefore, the prepared adhesive has strong adhesion, high mechanical strength, excellent water resistance and fire resistance.
[0021] The prepared adhesive material has a viscosity of 2010-2270 mPa•s, a water absorption of 7.23%-12.59%, a peel strength of 3.31-3.84 kN / mm, a tensile strength of 7.67-8.76 MPa, a toughness of 687-708%, and a thermal conductivity of 0.019-0.027 W / (m•K).
[0022] Beneficial effects obtained by the present invention:
[0023] 1. The present invention can greatly improve the cohesive force, mechanical strength, water resistance and fire resistance of the entire adhesive through cross-linking of the binary system of monocorn starch maleate and nitrile rubber.
[0024] 2. The adhesive prepared by the present invention has a simpler synthesis process than traditional adhesive materials, and the preparation method is environmentally friendly, safe, convenient, and low-cost. It can be widely used in the electronics industry, aerospace, chemical industry and other industries. DETAILED DESCRIPTION
[0025] The invention discloses a maleic acid monocorn starch ester modified nitrile rubber adhesive. The raw materials for preparing the maleic acid monocorn starch ester modified nitrile rubber adhesive include, by weight, 15-40 parts of corn starch, 30-60 parts of sodium hydroxide solution, 120-300 parts of anhydrous ethanol, 350-500 parts of acetone, 150-350 parts of methyl isobutyl ketone, 20-40 parts of maleic anhydride, 80-100 parts of nitrile rubber, 0.5-2 parts of zinc oxide, 0.5-2 parts of sulfur, 1-2 parts of carbon black, 1-4 parts of petroleum resin, 0.1-1 parts of antioxidant and 0.1-1 parts of coupling agent.
[0026] The corn starch is 20, 25 or 30 parts, sodium hydroxide solution is 50 parts, anhydrous ethanol is 200 parts, acetone is 400 parts, methyl isobutyl ketone is 200 parts, maleic anhydride is 27.5 parts, nitrile rubber is 100 parts, zinc oxide is 1 part, petroleum resin is 3 parts, sulfur is 1 part, carbon black is 1.5 parts, antioxidant is 0.5 parts and coupling agent is 0.5 parts. The mass fraction of the sodium hydroxide solution is 20%. The antioxidant is hydroquinone, hydroquinone dimethyl ether or propyl gallate, preferably, the antioxidant is hydroquinone. The coupling agent is a silane coupling agent. The solvent is one or more of anhydrous ethanol, acetone, butanone, methyl ethyl ketone, ethyl acetate, acetic acid, ethyl ester and methyl isobutyl ketone.
[0027] The present invention also discloses a method for preparing the aforementioned mono-corn starch maleate-modified nitrile rubber adhesive, comprising the following steps:
[0028] (1) Add corn starch, sodium hydroxide solution and anhydrous ethanol into a 100 mL three-necked flask at room temperature and reflux for 1.5-3 h. After cooling, wash with acetone solution and then filter. Then, place the sample in a 50 ℃ drying oven and dry it for 2-5 h to obtain activated corn starch.
[0029] (2) Pour the activated corn starch obtained in step (1) into a 100 mL three-necked flask, then slowly pour the acetone solution into the three-necked flask, stir magnetically at room temperature for 10-20 min, then heat and stir at 40-70 °C for 20-40 min.
[0030] (3) Add maleic anhydride to the acetone solution and stir until the maleic anhydride is completely dissolved; then slowly dropwise add the obtained maleic anhydride acetone solution into the three-necked flask in step (2); after the dropwise addition is completed, react at a constant temperature of 40-70°C for 4-6 hours; after the reaction is completed, cool the mixed solution, wash it with an acetone solution, and then filter it; place the filtered sample in a drying oven at 40-60°C and dry it to constant weight to obtain monocorn starch maleate.
[0031] (4) The nitrile rubber is plasticized on an open mixing mill with a roller distance of 2-3 mm for 1-5 min. Zinc oxide, carbon black, sulfur, petroleum resin, antioxidant and coupling agent are added in sequence for mixing. The roller distance is set to 0.5-2 mm. After the mixture is evenly mixed, the roller distance is adjusted to sheet the nitrile rubber.
[0032] (5) Using a shredder to shred the nitrile rubber sheet in step (4), pouring the shredded nitrile rubber sheet into a methyl isobutyl ketone solution, and mechanically stirring to dissolve the nitrile rubber sheet to obtain a uniform slurry, wherein the mechanical stirring speed is 800-1000 r / min.
[0033] (6) Slowly adding the monocorn starch maleate obtained in step (3) to the nitrile rubber mortar in step (5) under mechanical stirring at a speed of 800-1000 r / min for a stirring time of 30-50 min to obtain an adhesive mortar.
[0034] (7) The adhesive slurry prepared in step (6) is poured into a polytetrafluoroethylene mold and dried at 120° C. for 24 h to form an adhesive film, thereby obtaining a maleic acid monocorn starch ester-modified nitrile rubber adhesive.
[0035] The present invention is further described in detail with multiple embodiments below:
[0036] Embodiment 1:
[0037] At room temperature, 4g corn starch, 10g sodium hydroxide solution with a mass fraction of 20% and 40g anhydrous ethanol were added to a 100 mL three-necked flask for reflux reaction for 3 h. After cooling, they were washed with anhydrous ethanol and acetone respectively, and then filtered. Then the sample was placed in a drying oven at 50 °C for 3 h to obtain activated corn starch. The activated corn starch was poured into a 100mL three-necked flask, and then 20 mL acetone was slowly poured into the three-necked flask, magnetically stirred at room temperature for 15 min, and then the temperature was raised to 60 °C. 5.5g maleic anhydride was mixed with 20mL acetone at room temperature, and then magnetically stirred until the maleic anhydride was completely dissolved to obtain an acetone solution of maleic anhydride. Then the acetone solution of maleic anhydride was slowly added dropwise to the three-necked flask at a temperature of 60 °C, and the reaction was kept at a constant temperature for 6 hours after the addition was completed. After the reaction was completed, the mixed solution was cooled, then washed with acetone, and then filtered. The filtered sample was placed in a drying oven at 50° C. for 3 hours to obtain monocorn starch maleate.
[0038] 20g of nitrile rubber was plasticized on an open mill with a roller distance of 2-3 mm for 5 min, and then 0.2g of zinc oxide, 0.25g of carbon black, 0.2g of sulfur, 0.6g of petroleum resin, 0.1g of antioxidant and 0.1g of coupling agent were added in sequence for mixing, and the roller distance was set to 0.5-2 mm. After being mixed evenly, the roller distance was adjusted to sheet the nitrile rubber. The nitrile rubber film was shredded by a shredder, and the shredded nitrile rubber film was poured into a methyl isobutyl ketone solution, and then dissolved by mechanical stirring at 1000 r / min to obtain a uniform slurry. Then, maleic acid monocorn starch ester was slowly poured into the nitrile rubber slurry under mechanical stirring at a speed of 1000 r / min, and the stirring time was 45min. Then the slurry was poured into a polytetrafluoroethylene mold and dried at 120℃ for 24 h to form a film, and maleic acid monocorn starch ester modified nitrile rubber adhesive was obtained.
[0039] Embodiment 2:
[0040] At room temperature, 5 g corn starch, 10 g sodium hydroxide solution with a mass fraction of 20%, and 40 g anhydrous ethanol were added to a 100 mL three-necked flask for reflux reaction for 3 h. After cooling, the mixture was washed with anhydrous ethanol and acetone respectively, and then filtered. Then the sample was placed in a drying oven at 50 °C for 3 h to obtain activated corn starch. The activated corn starch was poured into a 100 mL three-necked flask, and then 20 mL acetone was slowly poured into the three-necked flask. The mixture was magnetically stirred for 15 min at room temperature, and then the temperature was raised to 60 °C. 5.5 g maleic anhydride was mixed with 20 mL acetone at room temperature, and then magnetically stirred until the maleic anhydride was completely dissolved to obtain an acetone solution of maleic anhydride. The acetone solution of maleic anhydride was then slowly added dropwise to the three-necked flask at 60 °C, and the mixture was kept at a constant temperature for 6 hours after the addition was completed. After the reaction was completed, the mixed solution was cooled, washed with acetone, and then filtered. The filtered sample was placed in a drying oven at 50° C. for 3 hours to obtain monocorn starch maleate.
[0041] 20 g of nitrile rubber was plasticized on an open mill with a roller distance of 2-3 mm for 5 min, and then 0.2 g zinc oxide, 0.25 g carbon black, 0.2 g sulfur, 0.6 g petroleum resin, 0.1 g antioxidant and 0.1 g coupling agent were added in sequence for mixing, and the roller distance was set to 0.5-2 mm. After being mixed evenly, the roller distance was adjusted to make the nitrile rubber sheet. The nitrile rubber film was shredded by a shredder, poured into a methyl isobutyl ketone solution, and then dissolved by mechanical stirring at 1000 r / min to obtain a uniform slurry. Then, maleic acid monocorn starch ester was slowly poured into the nitrile rubber slurry under mechanical stirring at a speed of 1000 r / min, and the stirring time was 45 min. Then the slurry was poured into a polytetrafluoroethylene mold and dried at 120°C for 24 h to form a film, and maleic acid monocorn starch ester modified nitrile rubber adhesive was obtained.
[0042] Embodiment 3:
[0043] At room temperature, 4 g corn starch, 10 g sodium hydroxide solution with a mass fraction of 20%, and 40 g anhydrous ethanol were added to a 100 mL three-necked flask for reflux reaction for 3 h. After cooling, the mixture was washed with anhydrous ethanol and acetone respectively, and then filtered. Then the sample was placed in a drying oven at 50 °C for 3 h to obtain activated corn starch. The obtained activated corn starch was poured into a 100 mL three-necked flask, and then 20 mL acetone was slowly poured into the three-necked flask, magnetically stirred at room temperature for 15 min, and then the temperature was raised to 60 °C. 5.5 g maleic anhydride was mixed with 20 mL acetone at room temperature, and then magnetically stirred until the maleic anhydride was completely dissolved to obtain an acetone solution of maleic anhydride. Then the acetone solution of maleic anhydride was slowly added dropwise to the three-necked flask at a temperature of 60 °C, and the reaction was kept at a constant temperature for 6 hours after the addition was completed. After the reaction was completed, the mixed solution was cooled, then washed with acetone, and then filtered. The filtered sample was placed in a drying oven at 50° C. for 3 hours to obtain monocorn starch maleate.
[0044] 20 g of nitrile rubber was plasticized on an open mill with a roller distance of 2-3 mm for 5 min, and then 0.2 g zinc oxide, 0.25 g carbon black, 0.2 g sulfur, 0.6 g petroleum resin, 0.1 g antioxidant and 0.1 g coupling agent were added in sequence for mixing, and the roller distance was set to 0.5-2 mm. After being mixed evenly, the roller distance was adjusted to make the nitrile rubber sheet. The nitrile rubber film was shredded by a shredder, poured into a methyl isobutyl ketone solution, and then dissolved by mechanical stirring at 1000 r / min to obtain a uniform slurry. Then, maleic acid monocorn starch ester was slowly poured into the nitrile rubber slurry under mechanical stirring at a speed of 1000 r / min, and the stirring time was 45 min. Then the slurry was poured into a polytetrafluoroethylene mold and dried at 120°C for 24 h to form a film, and maleic acid monocorn starch ester modified nitrile rubber adhesive was obtained.
[0045] Comparative Example 1:
[0046] 20 g of nitrile rubber was plasticized on an open mill with a roller distance of 2-3 mm for 5 min, and then 0.2 g of zinc oxide, 0.25 g of carbon black, 0.2 g of sulfur, 0.6 g of petroleum resin, 0.1 g of antioxidant and 0.1 g of coupling agent were added in sequence for mixing, and the roller distance was set to 0.5-2 mm. After the mixture was evenly mixed, the roller distance was adjusted to sheet the nitrile rubber. The nitrile rubber film was shredded by a shredder, and the shredded nitrile rubber film was poured into a methyl isobutyl ketone solution, and then a uniform slurry was obtained after mechanical stirring and dissolving at 1000 r / min. The slurry was then poured into a polytetrafluoroethylene mold and dried at 120°C for 24 h to form a film, thereby obtaining a nitrile rubber adhesive.
[0047] Comparative Example 2:
[0048] At room temperature, 5 g corn starch, 10 g sodium hydroxide solution (mass fraction) of 20%, and 40 g anhydrous ethanol were added to a 100 mL three-necked flask for reflux reaction for 3 h. After cooling, the mixture was washed with anhydrous ethanol and acetone respectively, and then filtered. The sample was then placed in a drying oven at 50 °C for 3 h to obtain activated corn starch.
[0049] 20 g of nitrile rubber was plasticized on an open mill with a roller distance of 2-3 mm for 5 min, and then 0.2 g zinc oxide, 0.25 g carbon black, 0.2 g sulfur, 0.6 g petroleum resin, 0.1 g antioxidant and 0.1 g coupling agent were added in sequence for mixing, and the roller distance was set to 0.5-2 mm. After being mixed evenly, the roller distance was adjusted to make the nitrile rubber sheet. The nitrile rubber film was shredded by a shredder, poured into a methyl isobutyl ketone solution, and then dissolved by mechanical stirring at 1000 r / min to obtain a uniform slurry. Then, activated corn starch was slowly poured into the nitrile rubber slurry under mechanical stirring at a speed of 1000 r / min, and the stirring time was 45 min. Then the slurry was poured into a polytetrafluoroethylene mold and dried at 120°C for 24 h to form a film, and a corn starch modified nitrile rubber adhesive was obtained.
[0050] Experimental performance test:
[0051] The viscosity test method is as follows:
[0052] 5 g of the adhesives of Examples 1-3 and Comparative Examples 1-2 were accurately weighed and placed in the sample box of the rapid viscosity analyzer. The measurement program was set as follows: the starting speed was 900 r / min, the speed was maintained at 150 r / min during the measurement, the measurement temperature was 25.0°C, and the measurement time was 10 min. After the measurement was completed, the viscosity value was read. In order to reduce the error, each sample was tested three times and then the average value was taken.
[0053] Table 1. The viscosity of Examples 1-3 and Comparative Examples 1-2 was tested, and the results are shown in the following table:
[0054] sample Temperature (℃) Viscosity (mPa·s) Example 1 25.0 2010 Example 2 25.0 2140 Example 3 25.0 2270 Comparative Example 1 25.0 600 Comparative Example 2 25.0 800
[0055] It can be seen from Table 1 that the viscosity values of Examples 1-3 are 2010 mPa•s, 2140 mPa•s and 2270 mPa•s, respectively; the viscosity values of Comparative Examples 1-2 are 600 mPa•s and 800 mPa•s, respectively; compared with Comparative Examples 1-2, it can be seen from Examples 1-3 that as the content of corn starch esterified with maleic anhydride increases from 20 wt% to 30 wt%, the viscosity value of the adhesive increases from 2010 mPa•s to 2270 mPa•s, indicating that the esterified corn starch can significantly increase the viscosity value of nitrile rubber. At the same time, as the content of corn starch esterified with maleic anhydride increases, the viscosity value of the adhesive is further increased.
[0056] Water resistance test:
[0057] The adhesive film was cut into 2 cm × 1 cm small squares, dried in a 60°C oven for 24 h, and then placed in a desiccator. The mass (m1) was weighed after cooling for 30 min, and then immersed in water at room temperature for 24 h. Subsequently, the expanded sample was taken out of the water, and the moisture on the surface of the sample was absorbed with filter paper and the mass (m2) was immediately weighed. The water absorption rate (%) was calculated as (m2 - m1) / m1× 100%.
[0058] Table 2 The water absorption rates of Examples 1-3 and Comparative Examples 1-2 were tested, and the results are shown in the following table:
[0059]
[0060] It can be seen from Table 2 that the water absorption rates of Examples 1-3 are in the range of 7.23%-12.59%; the water absorption rates of Comparative Examples 1-2 are between 20.52%-32.30%. It can be seen that as the content of corn starch esterified with maleic anhydride increases from 20wt% to 30wt%, the water absorption rate of the adhesive material decreases from 12.59% to 7.23%, and the water absorption rate of Example 3 is much lower than that of Comparative Examples 1-2, which proves that maleic anhydride monocorn starch ester can effectively reduce the water absorption rate of the adhesive and improve the water resistance of the adhesive.
[0061] Determination of peel strength, tensile strength, elongation at break, thermal conductivity:
[0062] The measurement was carried out according to the method specified in the national standard GB / T 7760-2003. The standard size is composed of an adhesive strip with a thickness of 5.0 mm ± 0.1 mm and a total length of about 75 mm bonded to a metal sheet. The surface of the metal sheet was polished with 2000-mesh sandpaper and then ultrasonically cleaned in an 80% ethanol solution to remove dust, grease and other impurities on the surface of the metal sheet, and then taken out and dried naturally. The adhesives of Examples 1-3 and Comparative Examples 1-2 were bonded to the surface-treated metal sheets, and then the bonded samples were heated in an oven at 60°C for 10 min. After that, the sample was taken out, and after the sample was completely cooled, it was pressed with a 20 kg weight for 2 min, and the peel strength (kN / mm) was measured with a universal tensile tester within 10 min.
[0063] According to the method specified in national standards GB 528-1998 and GB 528-1992, a dumbbell-shaped film of 75 mm × 4 mm × 1 mm was prepared, and the tensile strength and elongation at break of the film were tested at room temperature using a universal tensile testing machine at a tensile rate of 500 mm / min. To ensure accuracy, each sample should be measured at least three times in parallel and the average value should be taken.
[0064] Table 3 The peel strength, tensile strength, elongation at break and thermal conductivity of Examples 1-3 and Comparative Examples 1-2 were tested, and the results are shown in the following table:
[0065]
[0066] It can be seen from Table 3 that the peel strength of Examples 1-3 is between 3.31-3.84 kN / mm, the tensile strength is in the range of 7.67-8.76 (MPa), the elongation at break is between 687-708%, and the thermal conductivity is in the range of 0.019-0.027 W / (m•K); the peel strength of Comparative Examples 1-2 is between 0.63-0.86 kN / mm, the tensile strength is between 2.12-2.83 (MPa), and the elongation at break is between 654-688%. The thermal conductivity is between 0.052-0.061W / (m•K); therefore, in the preparation process of the maleic acid monocorn starch ester modified nitrile adhesive material of the present invention, the highly polar and highly active groups in the maleic acid monocorn starch ester macromolecular structure can react with metal oxides to form a complex, promote the adhesive and the metal surface to form a strong interaction, further improve the strength and adhesive performance of the adhesive, and the peel strength of the adhesive increases with the increase of the maleic acid monocorn starch ester content. At the same time, the hydroxyl and carboxyl groups of the maleic acid monocorn starch ester can also react with the cyanide in the nitrile rubber molecule, so that the maleic acid monocorn starch ester network and the nitrile rubber network form a whole, forming a double network structure, thereby greatly improving the reinforcing effect of the maleic acid monocorn starch ester on the nitrile rubber; therefore, the mechanical strength and fire resistance of the adhesive are further improved.
[0067] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.
Claims
1. A maleic acid monocorn starch ester modified nitrile rubber adhesive, characterized in that: The raw materials for preparing the maleic acid monocorn starch ester modified nitrile rubber adhesive include, by weight: 15-40 parts of corn starch, 30-60 parts of sodium hydroxide solution, 120-300 parts of anhydrous ethanol, 350-500 parts of acetone, 150-350 parts of methyl isobutyl ketone, 20-40 parts of maleic anhydride, 80-100 parts of nitrile rubber, 0.5-2 parts of zinc oxide, 0.5-2 parts of sulfur, 1-2 parts of carbon black, 1-4 parts of petroleum resin, 0.1-1 parts of antioxidant and 0.1-1 parts of coupling agent; the preparation method of the maleic acid monocorn starch ester includes the following steps: (1) Add corn starch, sodium hydroxide solution and anhydrous ethanol into a 100 mL three-necked flask at room temperature and reflux for 1.5-3 hours. After cooling, wash with acetone solution and then filter. Then, place the sample in a drying oven at 50° C. and dry for 2-5 hours to obtain activated corn starch. (2) pouring the activated corn starch obtained in step (1) into a 100 mL three-necked flask, then slowly pouring the acetone solution into the three-necked flask, stirring magnetically at room temperature for 10-20 min, then heating and stirring, the heating temperature is 40-70° C., and the stirring time is 20-40 min; (3) adding maleic anhydride to an acetone solution and stirring until the maleic anhydride is completely dissolved; then slowly dropping the obtained maleic anhydride acetone solution into the three-necked flask in step (2); after the dropping is complete, reacting at a constant temperature of 40-70° C. for 4-6 hours; after the reaction is completed, cooling the mixed solution, washing it with an acetone solution, and then filtering it; placing the filtered sample in a drying oven at 40-60° C. and drying it to constant weight, thereby obtaining monocorn starch maleate.
2. The mono-corn starch maleate modified nitrile rubber adhesive as claimed in claim 1, characterized in that: The corn starch is 20, 25 or 30 parts, sodium hydroxide solution is 50 parts, anhydrous ethanol is 200 parts, acetone is 400 parts, methyl isobutyl ketone is 200 parts, maleic anhydride is 27.5 parts, nitrile rubber is 100 parts, zinc oxide is 1 part, petroleum resin is 3 parts, sulfur is 1 part, carbon black is 1.5 parts, antioxidant is 0.5 parts and coupling agent is 0.5 parts.
3. The mono-corn starch maleate modified nitrile rubber adhesive as claimed in claim 1, characterized in that: The mass fraction of the sodium hydroxide solution is 20%.
4. The mono-corn starch maleate modified nitrile rubber adhesive as claimed in claim 1, characterized in that: The antioxidant is hydroquinone, hydroquinone dimethyl ether or propyl gallate.
5. The mono-corn starch maleate modified nitrile rubber adhesive as claimed in claim 1, characterized in that: The coupling agent is a silane coupling agent.
6. A method for preparing a mono-corn starch maleate-modified nitrile rubber adhesive as claimed in any one of claims 1 to 5, characterized in that: The following steps are included: (1) setting the roller distance of the nitrile rubber to 2-3 mm on an open mill for plasticizing, the plasticizing time is 1-5 min, then adding zinc oxide, carbon black, sulfur, petroleum resin, antioxidant and coupling agent in sequence for mixing, the roller distance is set to 0.5-2 mm, after the mixing is uniform, adjusting the roller distance to discharge the nitrile rubber; (2) using a shredder to shred the nitrile rubber film described in step (1), pouring the shredded nitrile rubber film into a methyl isobutyl ketone solution, and mechanically stirring to dissolve to obtain a uniform slurry, the mechanical stirring speed being 800-1000 r / min; (3) slowly adding monocorn starch maleate to the nitrile rubber mortar in step (2) under mechanical stirring, the mechanical stirring speed is 800-1000 r / min, and the stirring time is 30-50 min to obtain an adhesive mortar; (4) Pour the adhesive slurry in step (3) into a polytetrafluoroethylene mold and dry it at 120° C. for 24 h to form an adhesive film to obtain a maleic acid monocorn starch ester modified nitrile rubber adhesive.