A supercritical carbon dioxide drying device and its application and supercritical carbon dioxide drying method

Through the drying kettle arranged in parallel and the step-type carbon dioxide flow device, the problems of low drying efficiency and high energy consumption in the traditional supercritical carbon dioxide drying process are solved, and more efficient drying and lower energy consumption are achieved.

CN115704647BActive Publication Date: 2024-12-03IBIH ADVANCED MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110913059.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-10
Publication Date
2024-12-03
Estimated Expiration
2041-08-10

AI Technical Summary

Technical Problem

In the traditional supercritical carbon dioxide drying process, due to the constant carbon dioxide inflow method and flow rate, the drying efficiency is low, the energy consumption is high, and the solute cannot be completely brought out, which affects the product quality and efficiency.

Method used

The drying kettle and step-type carbon dioxide flow device are adopted to increase the drying efficiency and reduce energy consumption through feeding methods of up and down and out.

Benefits of technology

It improves drying efficiency, reduces energy consumption, and solves the problem that solute content decreases with the increase in the number of drying kettles, achieving more efficient drying and lower energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115704647B_ABST
    Figure CN115704647B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of supercritical drying, and discloses a supercritical carbon dioxide drying device and its application and a supercritical carbon dioxide drying method. The device comprises a supercritical treatment unit, a drying unit and a separation unit which are sequentially connected through a pipeline, wherein the drying unit contains 3-12 drying kettles arranged in parallel; the supercritical treatment unit is used to perform supercritical treatment on condensed carbon dioxide to obtain treated carbon dioxide; the drying unit is used to contact the treated carbon dioxide with a material to be dried to perform drying treatment to obtain an effluent I; the separation unit is used to separate the effluent I to obtain carbon dioxide and an effluent II that can be recycled. The supercritical carbon dioxide drying device and the drying method provided by the present invention have high drying efficiency and low energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of supercritical drying, in particular to a supercritical carbon dioxide drying device and application thereof in preparing aerogel, and a supercritical carbon dioxide drying method. Background Art

[0002] At present, the carbon dioxide in the traditional supercritical carbon dioxide drying process usually adopts the feeding method of bottom-in and top-out. The carbon dioxide flows into the drying kettle from the bottom and flows out from the top. Due to the influence of the gravity of the liquid matter in the material to be dried, the carbon dioxide cannot completely carry the liquid matter out of the drying kettle. The above problem can only be solved by increasing the extraction time, which leads to reduced work efficiency and increased energy consumption.

[0003] It is well known that supercritical carbon dioxide at a certain pressure and temperature has a certain solubility for solutes. However, in the prior art, drying kettles are usually connected in series. Since the solute cannot be completely removed by the carbon dioxide, this will inevitably lead to the carbon dioxide entering the next drying kettle containing a certain amount of solute, thereby reducing the amount of solute dissolved in the carbon dioxide in the next drying kettle. The more drying kettles there are, the more the amount of solute dissolved in the carbon dioxide gradually decreases, resulting in the product quality of the subsequent drying kettle being inferior to that of the previous drying kettle. The current solution to this problem is to increase the extraction time to ensure the qualified rate of the product, but this undoubtedly results in reduced efficiency and increased costs.

[0004] Meanwhile, the CO2 flow rate in traditional supercritical CO2 drying processes is typically kept constant. However, experiments have shown that in the early stages of drying, the material to be dried contains a high amount of liquid, so the initial CO2 introduced can remove a large amount of liquid. However, in the later stages of drying, the liquid content has significantly decreased, and maintaining a constant CO2 flow rate is meaningless. This undoubtedly results in waste and increased energy consumption. Summary of the Invention

[0005] The purpose of the present invention is to overcome the problems of low drying efficiency and high energy consumption in the prior art.

[0006] In order to achieve the above-mentioned object, the first aspect of the present invention provides a supercritical carbon dioxide drying device, which comprises:

[0007] A supercritical treatment unit, a drying unit, and a separation unit connected in sequence by pipelines, wherein the drying unit contains 3-12 drying kettles arranged in parallel;

[0008] The supercritical treatment unit is used to perform supercritical treatment on the condensed carbon dioxide to obtain treated carbon dioxide;

[0009] The drying unit is used to contact the treated carbon dioxide with the material to be dried to perform a drying process to obtain an effluent I;

[0010] The separation unit is used to separate the effluent I to obtain carbon dioxide and effluent II that can be recycled;

[0011] The pipelines in the drying units are arranged so that the treated carbon dioxide can be introduced from the upper portion of each drying kettle and led out from the lower portion of each drying kettle.

[0012] The second aspect of the present invention provides use of the supercritical carbon dioxide drying device described in the first aspect in preparing aerogel.

[0013] A third aspect of the present invention provides a supercritical carbon dioxide drying method, which is performed in the supercritical carbon dioxide drying device described in the first aspect, comprising:

[0014] (1) introducing the condensed carbon dioxide into a supercritical treatment unit for supercritical treatment to obtain treated carbon dioxide;

[0015] (2) introducing the treated carbon dioxide into each drying kettle arranged in parallel in the drying unit to contact with the material to be dried to perform a drying treatment, thereby obtaining an effluent I;

[0016] (3) The effluent I is introduced into a separation unit for separation to obtain carbon dioxide and effluent II that can be recycled.

[0017] The supercritical carbon dioxide drying device provided by the present invention has the following beneficial effects:

[0018] (1) The supercritical carbon dioxide drying device provided by the present invention adopts a top-in and bottom-out feeding method, which can convert the gravity of the solute from resistance into power.

[0019] (2) The drying kettles in the supercritical carbon dioxide drying device provided by the present invention are connected in parallel, so that each drying kettle works independently, which can effectively solve the problem that the solute content in carbon dioxide decreases as the number of drying kettles increases, thereby improving the drying efficiency.

[0020] (3) The supercritical carbon dioxide drying device provided by the present invention can adopt a step-by-step carbon dioxide flow rate method to gradually reduce the carbon dioxide flow rate, thereby reducing energy consumption.

[0021] (4) The supercritical carbon dioxide drying device provided by the present invention has the advantage of adjustable production scale and can be adjusted according to actual production conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a diagram of a supercritical carbon dioxide drying device in a preferred embodiment provided by the present invention.

[0023] Description of Reference Numerals

[0024] Y1-Storage unit E1-Condensation unit I P1-Pressure pump E2-Heat exchanger I

[0025] R1-Drying kettle R2-Drying kettle R3-Drying kettle

[0026] E3-Heat exchanger II S1-Separation kettle E4-Heat exchanger II S2-Separation kettle

[0027] Y2- Recovery unit I Y3- Recovery unit II C1 compression pump E5- Condensation unit II DETAILED DESCRIPTION

[0028] The endpoints of the ranges and any values ​​disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered to be specifically disclosed herein.

[0029] As mentioned above, the first aspect of the present invention provides a supercritical carbon dioxide drying device, which includes:

[0030] A supercritical treatment unit, a drying unit, and a separation unit connected in sequence by pipelines, wherein the drying unit contains 3-12 drying kettles arranged in parallel;

[0031] The supercritical treatment unit is used to perform supercritical treatment on the condensed carbon dioxide to obtain treated carbon dioxide;

[0032] The drying unit is used to contact the treated carbon dioxide with the material to be dried to perform a drying process to obtain an effluent I;

[0033] The separation unit is used to separate the effluent I to obtain carbon dioxide and effluent II that can be recycled;

[0034] The pipelines in the drying units are arranged so that the treated carbon dioxide can be introduced from the upper portion of each drying kettle and led out from the lower portion of each drying kettle.

[0035] The inventors of the present invention have found that, compared with the prior art, the drying device provided by the present invention has higher drying efficiency and lower energy consumption.

[0036] Preferably, the drying unit comprises three drying kettles arranged in parallel.

[0037] Preferably, the supercritical treatment unit comprises a pressure pump and a heat exchanger I connected in sequence. It should be noted that the present invention does not particularly limit the number of the pressure pump and the heat exchanger I. Those skilled in the art can select them in combination with known techniques in the art. The present invention will not be described in detail here, and those skilled in the art should not be construed as limiting the present invention. The present invention exemplarily provides a preferred embodiment. In order to achieve higher drying efficiency and lower energy consumption, the number of the pressure pump and the heat exchanger I in the present invention is 1 respectively, and a series connection method is adopted with the pressure pump in front and the heat exchanger I in the back.

[0038] Preferably, the separation unit comprises a heat exchanger II and a separation kettle which are connected in sequence, and the heat exchanger II is connected to the drying kettle.

[0039] Further preferably, the number of the heat exchangers II is at least 2, and the number of the separation kettles is at least 2. In the present invention, the two heat exchangers II and the two separation kettles can be connected in series: the heat exchanger II, the separation kettle, the heat exchanger II, and the separation kettle, wherein the heat exchanger II is connected to the drying kettle.

[0040] Preferably, the device further comprises a recovery unit I and a recovery unit II, wherein the recovery unit I is arranged downstream of the separation unit and is connected to the separation kettle, and the recovery unit II is arranged in parallel with the separation unit downstream of the drying unit, the recovery unit I is used to recover the effluent II, and the recovery unit II is used to recover a portion of the carbon dioxide that can be recycled.

[0041] Preferably, the device further comprises a storage unit disposed upstream of the supercritical treatment unit, wherein the storage unit is capable of storing carbon dioxide.

[0042] According to a preferred embodiment, the device further includes a condensation unit I disposed between the storage unit and the supercritical treatment unit, and the condensation unit I is used to condense the carbon dioxide drawn out from the storage unit.

[0043] According to another preferred embodiment, the device further includes a condensing unit II arranged between the storage unit and the recovery unit II, and the condensing unit II is used to condense the remaining part of the recyclable carbon dioxide, and the raw material condensed by the condensing unit II is circulated back to the storage unit.

[0044] It should be noted that the present invention has no particular limitation on the types of drying kettle, separation kettle, and heat exchanger. Those skilled in the art can make their selections based on known technologies in the art. The present invention will not be described in detail herein, and those skilled in the art should not interpret this as a limitation on the present invention.

[0045] It should be noted that the present invention has no particular restrictions on the type and quantity of equipment used in the storage unit, condensing unit, and recovery unit. Those skilled in the art can make selections based on known technologies in the art. The present invention will not be described in detail here, and those skilled in the art should not understand this as a limitation of the present invention.

[0046] It should be noted that various control valves known to those skilled in the art may be provided in the circulation passage of the device of the present invention to control the flow of the carbon dioxide fluid.

[0047] It should be noted that all pressure vessels in the device of the present invention (e.g., storage unit, drying kettle, separation kettle, heat exchanger, condensing unit) can be equipped with independent drain valves, and can also be equipped with pressure gauges and thermometers to display the pressure and temperature within the device. The carbon dioxide storage unit and the carbon dioxide recovery unit can also be equipped with a carbon dioxide volume meter to display the volume of liquid carbon dioxide in the device. Each drying kettle can be equipped with a flow meter to display the flow rate of carbon dioxide introduced into each drying kettle. In order to achieve the circulation process, the various devices in the device of the present invention can be arranged or set to match each other according to specific needs.

[0048] It should be noted that a material capable of adsorbing the solvent (the solvent in the material to be dried), including but not limited to molecular sieves, may be placed in the separation kettle in the device of the present invention, and the material is regularly replaced and activated.

[0049] The following combination Figure 1 The supercritical carbon dioxide drying device of the present invention is exemplified.

[0050] Carbon dioxide feedstock is drawn from storage unit Y1 and introduced into condensation unit I E1 for condensation treatment I. The condensed carbon dioxide is introduced into pressure pump P1 for pressurization treatment. The pressurized carbon dioxide is introduced into heat exchanger I E2 for heating treatment to obtain supercritical carbon dioxide. The supercritical carbon dioxide is introduced into drying kettles R1, R2, and R3, respectively, for drying treatment with the material to be dried contained therein (they can be introduced simultaneously or individually). After drying, the carbon dioxide carrying the solvent is introduced into heat exchanger II E3 and / or heat exchanger II E4 for heating treatment. After heating treatment, it is introduced into separation kettle S1 and / or separation kettle S2 for separation. The separated effluent II is introduced into recovery unit I Y2 for recovery treatment. A portion of the recyclable carbon dioxide is introduced into recovery unit II Y3, and the remaining portion is compressed by compression pump C1 and introduced into condensation unit II E5 for condensation treatment II. The carbon dioxide after condensation treatment II is recycled back to storage unit Y1 for reuse. Among them, the carbon dioxide in the recovery unit IIY3 can be compressed by the compression pump C1 when the device is not in operation and then introduced into the condensation unit II E5 for condensation treatment II, and the carbon dioxide after condensation treatment II is introduced into the storage unit Y1 for recycling.

[0051] As mentioned above, the second aspect of the present invention provides the use of the supercritical carbon dioxide drying device described in the first aspect in preparing aerogel.

[0052] As mentioned above, the third aspect of the present invention provides a supercritical carbon dioxide drying method, which is carried out in the supercritical carbon dioxide drying device described in the first aspect, comprising:

[0053] (1) introducing the condensed carbon dioxide into a supercritical treatment unit for supercritical treatment to obtain treated carbon dioxide;

[0054] (2) introducing the treated carbon dioxide into each drying kettle arranged in parallel in the drying unit to contact with the material to be dried to perform a drying treatment, thereby obtaining an effluent I;

[0055] (3) The effluent I is introduced into a separation unit for separation to obtain carbon dioxide and effluent II that can be recycled.

[0056] Preferably, the method further comprises, before performing step (1), introducing the carbon dioxide feedstock in the storage unit into a condensation unit I for condensation treatment I to obtain the condensed carbon dioxide. The purpose of the condensation treatment I is to prevent the carbon dioxide from vaporizing, thereby ensuring that the pressure pump can deliver the carbon dioxide to each of the drying kettles.

[0057] According to a preferred embodiment, the method further comprises, after performing step (3), introducing the effluent II into a recovery unit I for recovery treatment, introducing a portion of the recyclable carbon dioxide into the recovery unit II, and recycling the remaining portion of the recyclable carbon dioxide back to the condensation unit II for condensation treatment II, and introducing the material obtained after the condensation treatment II into the storage unit.

[0058] Preferably, the volume ratio of the portion of the recyclable carbon dioxide to the remaining portion of the recyclable carbon dioxide is 1:0.83-0.95. The inventors of the present invention have found that under this preferred embodiment, the drying method provided by the present invention has lower energy consumption.

[0059] According to another preferred embodiment, in step (2), the drying conditions in each drying kettle are the same or different, and each independently satisfies at least: controlling the flow rate of the treated carbon dioxide to 800-1500 L / h.

[0060] In order to achieve higher drying efficiency and lower energy consumption, preferably, the drying conditions in each drying kettle independently meet at least the following conditions:

[0061] When the drying process is performed for 0-2 hours, the flow rate of the treated carbon dioxide is controlled to be 1200-1500 L / h;

[0062] When the drying process is performed for 2-4 hours, the flow rate of the treated carbon dioxide is controlled to be 1000-1200 L / h;

[0063] When the drying process is performed for 4-6 hours, the flow rate of the carbon dioxide after the treatment is controlled to be 800-1000 L / h.

[0064] It should be noted that there are no particular limitations on the pressures and temperatures of the storage unit, drying unit, and separation unit in the apparatus of the present invention. For example, the pressure in the storage unit may be 4-5 MPa and the temperature may be 7-15°C; the pressure in the drying unit may be 13-16 MPa and the temperature may be 50-70°C; and the pressure in the separation unit may be 4-8 MPa and the temperature may be 40-60°C.

[0065] It should be noted that all timings in the present invention start from the time when the inlet valve of the drying kettle is opened to begin introducing the treated carbon dioxide. When the drying process is performed for 0-2 hours, it means from the time when the inlet valve of the drying kettle is opened to begin introducing the treated carbon dioxide to the time when the treated carbon dioxide is introduced for 2 hours. Similarly, when the drying process is performed for 2-4 hours, it means from the time when the treated carbon dioxide is introduced for 2 hours to the time when the treated carbon dioxide is introduced for 4 hours. Those skilled in the art can infer the same thing, and the present invention will not be repeated here.

[0066] The drying process in the present invention preferably adopts intermittent drying process, that is, after the product is dried, the inlet valve of the drying kettle is temporarily closed to carry out the loading and unloading process of the product.

[0067] The present invention will be described in detail below through examples.

[0068] In the following examples, the method for preparing the wet gel to be dried is as follows: the wet gel to be dried is prepared by referring to the method in Example 1 in CN103118979A.

[0069] Carbon dioxide storage tank: volume is 10m 3 .

[0070] Carbon dioxide drying kettle: volume is 3m 3 .

[0071] Separation kettle: volume is 3m 3 .

[0072] Solvent recovery tank: volume 1m 3 .

[0073] Carbon dioxide recovery tank: volume is 3m 3 .

[0074] Example 1

[0075] The wet gel to be dried of 750L is placed in each drying kettle, the carbon dioxide after condensation process is introduced in each drying kettle, carry out drying process, after drying process is complete, effluent I is introduced into separating kettle after cooling and decompression process and carries out separation process, when the solvent level in solvent recovery tank reaches setting liquid level (4 / 5 place of equipment volume), carry out solvent recovery process, after separation process finishes, drying kettle first carries out pressure balance with carbon dioxide storage tank, a part of carbon dioxide is carried out compression and condensation process and then circulates back to carbon dioxide storage tank, then carries out pressure balance with carbon dioxide recovery tank, remainder carbon dioxide is introduced into carbon dioxide storage tank, wherein, the carbon dioxide in carbon dioxide recovery tank can be compressed and condensed and be introduced into carbon dioxide storage tank when equipment is not running.And calculate drying efficiency and energy consumption.Wherein, the condition parameters in each device and the parameter of drying process technology are all listed in Table 1, and the result of drying efficiency and energy consumption is listed in Table 2.

[0076] Examples 2-6

[0077] Examples 2-6 were carried out using a method similar to that of Example 1, except that the conditions and parameters of the apparatus and the drying process were different, which are specifically listed in Table 1. The results are listed in Table 2.

[0078] Comparative Example 1

[0079] This comparative example was carried out using a method similar to Example 1, except that the pipeline settings were adjusted so that the treated carbon dioxide was introduced from the lower part of the drying kettle and drawn out from the upper part of the drying kettle. Specific drying conditions are shown in Table 1, and the results are shown in Table 2.

[0080] Comparative Example 2

[0081] This comparative example was carried out using a method similar to that of Example 1, except that the connection mode of the drying kettles was adjusted so that the drying kettles were connected in series, and the carbon dioxide entering the next drying kettle was drawn out from the previous drying kettle. Specific drying conditions are shown in Table 1, and the results are shown in Table 2.

[0082] Comparative Example 3

[0083] This comparative example was carried out using a method similar to that of Example 1, except that the connection method of the drying kettles was adjusted so that the drying kettles were connected in series, and the carbon dioxide entering the next drying kettle was drawn out from the previous drying kettle. At the same time, the setting of the pipeline was adjusted so that the treated carbon dioxide was introduced from the bottom of the drying kettle and drawn out from the top of the drying kettle. Specific drying conditions are shown in Table 1, and the results are shown in Table 2.

[0084] Drying efficiency: the weight of solvent recovered per unit time, in kg / h.

[0085] Table 1

[0086]

[0087]

[0088] Table 1

[0089]

[0090]

[0091] Table 2

[0092]

[0093]

[0094] It can be seen from the results in Table 2 that the supercritical carbon dioxide drying device and drying method provided by the present invention have higher drying efficiency and lower energy consumption.

[0095] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, various simple variations of the technical solution of the present invention may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed in the present invention and fall within the scope of protection of the present invention.

Claims

1. A supercritical carbon dioxide drying method, It is characterized in that The method is carried out in a supercritical carbon dioxide drying device, comprising: The supercritical carbon dioxide drying device comprises a supercritical treatment unit, a drying unit and a separation unit which are sequentially connected through pipelines, and the drying unit contains 3-12 drying kettles arranged in parallel; The arrangement of the pipelines in the drying unit enables the treated carbon dioxide to be introduced from the upper part of each drying kettle and led out from the lower part of each drying kettle; The supercritical treatment unit comprises a pressure pump and a heat exchanger I which are connected in sequence, and a series connection mode is adopted in which the pressure pump is in front and the heat exchanger I is in the back; (1) introducing the condensed carbon dioxide into a supercritical treatment unit for supercritical treatment to obtain treated carbon dioxide; (2) introducing the treated carbon dioxide into each drying kettle arranged in parallel in the drying unit to contact with the material to be dried to perform drying treatment, thereby obtaining effluent I; (3) introducing the effluent I into a separation unit for separation to obtain carbon dioxide and effluent II that can be recycled; In step (2), the drying conditions in each drying kettle independently satisfy at least: When the drying process is performed for 0-2 hours, the flow rate of the carbon dioxide after the treatment is controlled to be 1200-1500 L / h; When the drying process is performed for 2-4 hours, the flow rate of the treated carbon dioxide is controlled to be 1000-1200 L / h; When the drying process is performed for 4-6 hours, the flow rate of the carbon dioxide after the process is controlled to be 800-1000 L / h.

2. The method according to claim 1, in, The drying unit comprises three drying kettles arranged in parallel.

3. The method according to claim 1, in, The separation unit comprises a heat exchanger II and a separation kettle which are connected in sequence, and the heat exchanger II is connected to the drying kettle.

4. The method according to claim 3, in, The number of the heat exchangers II is at least 2, and the number of the separation kettles is at least 2.

5. The method according to claim 2, in, The device also includes a recovery unit I and a recovery unit II, wherein the recovery unit I is arranged downstream of the separation unit and is connected to the separation kettle, and the recovery unit II is arranged in parallel with the separation unit downstream of the drying unit, the recovery unit I is used to recover the effluent II, and the recovery unit II is used to recover a portion of the carbon dioxide that can be recycled.

6. The method according to any one of claims 1 to 5, in, The device further comprises a storage unit disposed upstream of the supercritical treatment unit, wherein the storage unit is capable of storing carbon dioxide.

7. The method according to claim 6, in, The device also includes a condensation unit I disposed between the storage unit and the supercritical processing unit, and the condensation unit I is used to condense the carbon dioxide drawn out from the storage unit.

8. The method according to claim 6, in, The device further comprises a condensing unit II disposed between the storage unit and the recovery unit II, wherein the condensing unit II is used to condense the remaining portion of the carbon dioxide that can be recycled.

9. The method according to claim 1, in, The method further comprises, before performing the step (1), first introducing the carbon dioxide raw material in the storage unit into a condensation unit I for condensation treatment I to obtain the condensed carbon dioxide.

10. The method according to claim 1, in, The method further comprises, after performing the step (3), introducing the effluent II into a recovery unit I for recovery treatment, introducing a portion of the recyclable carbon dioxide into the recovery unit II, and recycling the remaining portion of the recyclable carbon dioxide back to the condensation unit II for condensation treatment II, and introducing the material obtained after the condensation treatment II into a storage unit.