A hexagonal photocatalyst and its preparation method
A highly crystalline hexagonal prism-shaped photocatalyst was prepared by recrystallizing graphite-phase carbon nitride using a microwave-assisted hot solvent method, which solved the problems of difficult charge transfer and low nitrogen activation efficiency of traditional g-C3N4 photocatalysts, and achieved efficient photocatalysis. The ability to react with nitrogen fixation and oxidize nitrogen to generate nitrate radicals is significantly improved.
Patent Information
- Application Number
- CN202211504183.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-11-29
AI Technical Summary
In the traditional thermal polymerization synthesis method, the existing graphite phase carbon nitride (g-C3N4) photocatalyst has insufficient mobility of the reaction intermediate, resulting in an amorphous structure, difficulty in charge transfer, low photogenerated carrier separation rate, and in nitrogen gas The product during the activation process is mainly NH3, which lacks the ability to efficiently oxidize nitrogen.
Microwave-assisted hot solvent recrystallization of ultrathin g-C3N4 was used to prepare hexagonal prism photocatalyst (CCN), and its crystallization was improved by using ethyl acetate-carbon tetrachloride azeotropic mixture and ethylene dioleic acid amide surfactant. properties and surface hydroxyl group content, enhancing the π-conjugated electron concentration and carrier lifetime.
The photocatalytic performance of CCN is significantly improved. The rate of photocatalytic nitrogen fixation to generate nitrate reaches 34.56mgh-1g-1, which is much higher than that of traditional PCN. In addition, with the participation of oxygen, N2 activation and oxygen reaction are realized, and the ability to generate nitrate is significantly improved. improve.
Smart Images

Figure CN115709092B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of semiconductor photocatalysis, and specifically relates to a hexagonal g-C3N4 photocatalyst and a preparation method thereof. Technical Background
[0002] In recent years, researchers have gradually begun to explore metal-free and efficient photocatalysts. Graphene-phase carbon nitride (g-C3N4) has entered the field of vision of researchers due to its simple composition, special electronic structure, visible light absorption, and stable physical and chemical properties. In the traditional thermal polymerization synthesis method, due to the insufficient mobility of the reaction intermediates, g-C3N4 cannot be completely polymerized, resulting in an amorphous structure. This amorphous structure makes it difficult for charges to transfer on the conjugated aromatic ring plane of g-C3N4, which is manifested as a very low separation rate of photogenerated carriers inside g-C3N4.
[0003] Researchers have adopted many modification methods to improve the photocatalytic performance of g-C3N4. Enhancing the crystallinity of g-C3N4 is also an important means to affect its photocatalytic performance. Because the crystallinity is enhanced, the azine ring structure in the system is not easy to break, which means that the π electron conjugated system inside the system will be more complete and have more delocalized π conjugated electrons. This feature is conducive to accelerating the transfer of its photogenerated charge. In addition, the internal long-range order will reduce the recombination center of the electron, further improving its photocatalytic performance. In addition, the introduction of defects in g-C3N4 is considered by researchers to be an important means to improve the photocatalytic performance. The introduction of structural defects can change its electronic structure, band structure, carrier state, etc., and can increase the number of active sites for the reaction. In addition, surface hydroxylation is also an effective modification method that can greatly improve its photocatalytic performance, which can accelerate the transfer of interface electrons. On the basis of introducing C defects, further increasing the number of surface hydroxyl groups can improve the oxidation performance of the photocatalyst. Since Schrauzer et al. reported in 1977 that nitrogen fixation can be achieved through photocatalysis, photocatalysis has been widely used in the field of nitrogen fixation because it is efficient and sustainable, and can achieve nitrogen fixation at room temperature and pressure. However, in existing research, the product of nitrogen activation by g-C3N4 is mostly NH3, which is only the first step in the process of industrial preparation of nitric acid. Liu et al. have realized the direct photocatalytic generation of NO3 from N2 using WO3 - At the same time, g-C3N4 has also been widely used in the oxidation process of NO. NO is one of the products in the oxidation process of N2. Therefore, in the present invention, it is possible to try to use g-C3N4 to activate N2 in the presence of oxygen, and make it react with oxygen to generate nitrate.
[0004] Based on this, the present invention adopts a microwave-assisted thermal solvent method to prepare hexagonal g-C3N4 (CCN) with enhanced crystallinity by recrystallizing ultra-thin g-C3N4, and compared with PCN, CCN introduces a large number of hydroxyl groups on its surface. In addition, the conjugated structure of CCN has a higher concentration of π-conjugated electrons, and the lifetime of the carriers inside CCN is longer than that of PCN. On this basis, the invention uses photocatalytic nitrogen fixation to produce nitrate as a model reaction, which shows that the rate of CCN photocatalytic nitrogen fixation to produce nitrate is also greatly improved, which can reach 34.56 mg / L. -1 g -1 , which is much higher than the rate at which PCN produces nitrate. Summary of the invention
[0005] A hexagonal prism-shaped photocatalyst has a hexagonal prism-shaped microstructure, a diameter of 1 to 3 μm, and rich hydroxyl functional groups on its surface.
[0006] The present invention also provides a method for preparing a hexagonal photocatalyst, which is prepared by using ultrathin graphite phase carbon nitride g-C3N4 as a raw material, an ethyl acetate-carbon tetrachloride azeotropic mixture as a solvent, and ethylene dioleic acid amide as a surfactant, and adopting a microwave-assisted recrystallization method.
[0007] Furthermore, the method for preparing the hexagonal prism-shaped photocatalyst comprises the following steps:
[0008] (1) Urea is placed in an alumina crucible and placed in a muffle furnace. The heating rate and target temperature are controlled and kept warm for a certain period of time. After natural cooling, a light yellow sample is obtained, which is marked as UCN.
[0009] (2) UCN was placed in an open crucible and placed in a muffle furnace for secondary quenching to obtain a white powder sample, which was labeled as PCN;
[0010] (3) placing PCN in a beaker, adding ethyl acetate-carbon tetrachloride azeotropic mixture, and then adding ethylene dioleic acid amide surfactant, and performing high-power ultrasonic stirring to obtain a uniform mixed suspension;
[0011] (4) The suspension was placed in a reactor for hydrothermal reaction. After natural cooling, the sample was washed three times with water and ethanol respectively, and separated using a centrifuge.
[0012] (5) The washed sample was vacuum freeze-dried to obtain a powdered hexagonal photocatalyst sample, which was labeled as CCN.
[0013] Furthermore, in step (1), the mass of urea is 10 g, the heating rate is 5° C. / min, the target temperature is 550° C., and the holding time is 3 hours.
[0014] Furthermore, in step (2), the secondary annealing treatment has a heating rate of 20°C / min, a target temperature of 600°C, a holding time of 2 hours, and then quenching at room temperature.
[0015] Furthermore, the mass ratio of the ethyl acetate-carbon tetrachloride azeotropic mixture in step (3) is 43:57, and the total volume is 40 mL.
[0016] Furthermore, the mass fraction of the ethylene dioleic acid amide surfactant in step (3) is 1.5%, the ultrasonic power is 200 W, and the ultrasonic dispersion time is 2 days.
[0017] Furthermore, in the hydrothermal reaction of step (4), the volume of the reactor liner is 50 mL, the material is PPL, and the hydrothermal conditions are to keep warm at 120-240° C. for 6-12 hours.
[0018] Furthermore, the vacuum degree of the vacuum freeze-drying in step (5) is <15Pa, the temperature is <-50°C, and the time is 24 hours.
[0019] The present invention is beneficial in that:
[0020] The present invention uses microwave-assisted thermal solvent method to recrystallize g-C3N4 (PCN) to prepare a hexagonal g-C3N4 photocatalyst (CCN) with enhanced crystallinity. Hydroxyl groups are also introduced on the surface of CCN. Among them, CCN has better crystallinity than PCN, and the internal azine ring plane is more complete, which can produce a large number of delocalized π electrons, its fluorescence lifetime becomes longer, and the carrier recombination efficiency becomes lower. Due to the higher crystallinity of CCN, the electron and hole transfer rate will be faster. The results show that CCN photocatalytic nitrogen fixation produces NO3 - The rate is much higher than that of PCN. Therefore, the present invention improves the crystallinity of g-C3N4 through modification, improves the generation, transfer and recombination process of its photogenerated carriers, and significantly improves its photocatalytic performance. This provides a new idea for the design of photocatalytic materials and a new possible way for the direct oxidation of nitrogen to generate nitrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Scanning electron microscope images of (a) hexagonal g-C3N4 photocatalyst (CCN) and (b) PCN prepared in Example 1 of the present invention;
[0022] Figure 2 X-ray diffraction patterns of PCN and CCN prepared in Example 1 of the present invention;
[0023] Figure 3 (a) Full XPS spectra of CCN and PCN prepared in Example 1 of the present invention, and high-resolution (b) C 1s (c) N 1s (d) FTIR spectra;
[0024] Figure 4 (a) UV-visible diffuse reflectance spectra and (b) Tauc curves of PCN and CCN prepared in Example 1 of the present invention;
[0025] Figure 5 PCN and CCN prepared in Example 1 of the present invention (a) Photocatalytic nitrate production graph under air conditions (b) and nitrate rate graph (c) Blank control under argon conditions (d) 15 N isotope abundance (e) Ion chromatogram data of PCN (f) Ion chromatogram data of CCN.
[0026] Specific implementation cases
[0027] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below with reference to the accompanying drawings.
[0028] Example 1
[0029] A method for preparing a hexagonal g-C3N4 (CCN) photocatalyst comprises the following steps:
[0030] (1) 10 g of urea was placed in an alumina crucible and placed in a muffle furnace. The heating rate was set to 5 °C / min, the target temperature was 550 °C, and the holding time was 3 hours. After natural cooling, a light yellow sample was obtained, which was marked as UCN.
[0031] (2) UCN was placed in an open crucible and placed in a muffle furnace for secondary quenching treatment at a heating rate of 20 °C / min, a target temperature of 600 °C, and a holding time of 2 h. Then, it was quenched at room temperature to obtain a white powder sample, which was labeled as PCN.
[0032] (3) 30 mg of PCN was placed in a beaker, 40 mL of ethyl acetate-carbon tetrachloride azeotropic mixture (mass ratio of 43:57) was added, and then 1.5% of ethylene dioleic acid amide surfactant was added, and ultrasonic stirring was performed at an ultrasonic power of 200 W for 2 days to obtain a uniform mixed suspension;
[0033] (4) The suspension was placed in a reactor for hydrothermal reaction. The volume of the reactor was 50 mL and the material was PPL. The hydrothermal temperature was 180°C and the reaction was kept for 6 hours. After natural cooling, the sample was washed 3 times with water and ethanol respectively and separated by a centrifuge.
[0034] (5) The washed sample was subjected to vacuum freeze drying and thoroughly dried in a vacuum drying oven with a vacuum degree of <15 Pa and a temperature of <-50°C for 24 hours to obtain a white powder sample, which was marked as CCN.
[0035] Figure 1 The scanning electron microscope images of the hexagonal g-C3N4 photocatalyst (CCN) and PCN prepared in Example 1 of the present invention show that PCN is a common g-C3N4 structure, both showing a flaky morphology and containing a large number of pore structures between the lamellae. Figure 1 b is the SEM image of CCN. It can be seen that regular hexagonal prism-like structures appear in the structure of CCN, which indicates that part of the lamellar structure is reconstructed and transformed into hexagonal prisms.
[0036] Figure 2 The X-ray diffraction diagrams of PCN and CCN prepared in Example 1 of the present invention show that both PCN and CCN prepared in the present invention are carbon nitrides with graphite phase structures, but compared with common PCN, CCN has a higher long-range order and stronger crystallinity in its internal structure. This feature is conducive to the rapid transmission of its internal carriers.
[0037] Figure 3 (a) The XPS full spectrum of CCN and PCN prepared in Example 1 of the present invention, as well as the high-resolution (b) C 1s (c) N 1s (d) FTIR spectra, it can be seen that after reconstruction, the structure of CCN has not changed significantly compared with PCN, but due to the high temperature treatment during the solvent thermal treatment, more hydroxyl groups are adsorbed on the surface of CCN.
[0038] Figure 4 (a) UV-visible diffuse reflectance spectra and (b) Tauc curves of PCN and CCN prepared in Example 1 of the present invention. It can be seen that after high-temperature solvent thermal reconstruction, the light absorption band edge of CCN shows an obvious blue shift, the band gap width of CCN is larger than that of PCN, and its light absorption ability is weakened compared with PCN. This is due to the change in its morphology and the hydroxyl groups on the surface.
[0039] Figure 5 PCN and CCN prepared in Example 1 of the present invention (a) Photocatalytic nitrate production graph under air conditions (b) and nitrate rate graph (c) Blank control under argon conditions (d) 15 N isotope abundance (e) ion chromatography data of PCN (f) ion chromatography data of CCN. It can be seen that the nitrate production of CCN gradually increases with time and presents an approximately linear relationship, indicating that the increase in the content of nitrate within a certain period of time is certain. On the contrary, the nitrate production of PCN has not increased significantly, indicating that the ability of CCN to photocatalyze nitrogen to produce nitrate is much higher than that of PCN. Moreover, CCN photocatalytic nitrogen fixation produces NO3 - The rate is much higher than PCN.
[0040] Example 2
[0041] A method for preparing a hexagonal g-C3N4 (CCN) photocatalyst comprises the following steps:
[0042] (1) 10 g of urea was placed in an alumina crucible and placed in a muffle furnace. The heating rate was set to 5 °C / min, the target temperature was 550 °C, and the holding time was 3 hours. After natural cooling, a light yellow sample was obtained, which was marked as UCN.
[0043] (2) UCN was placed in an open crucible and placed in a muffle furnace for secondary quenching treatment at a heating rate of 5 °C / min, a target temperature of 600 °C, a holding time of 2 h, and then naturally cooled at room temperature to obtain a powder sample, which was labeled as PCN;
[0044] (3) 30 mg of PCN was placed in a beaker, 40 mL of ethyl acetate-carbon tetrachloride azeotropic mixture (mass ratio of 43:57) was added, and then 1.5% of ethylene dioleic acid amide surfactant was added, and ultrasonic stirring was performed at an ultrasonic power of 200 W for 2 days to obtain a uniform mixed suspension;
[0045] (4) The suspension was placed in a reactor for hydrothermal reaction. The volume of the reactor was 50 mL and the material was PPL. The hydrothermal temperature was 180°C and the reaction was kept for 6 hours. After natural cooling, the sample was washed 3 times with water and ethanol respectively and separated by a centrifuge.
[0046] (5) The washed sample was subjected to vacuum freeze drying and thoroughly dried in a vacuum drying oven with a vacuum degree of <15 Pa and a temperature of <-50°C for 24 hours to obtain a white powder sample, which was marked as CCN.
[0047] Example 3
[0048] A method for preparing a hexagonal g-C3N4 (CCN) photocatalyst comprises the following steps:
[0049] (1) 10 g of urea was placed in an alumina crucible and placed in a muffle furnace. The heating rate was set to 5 °C / min, the target temperature was 550 °C, and the holding time was 3 hours. After natural cooling, a light yellow sample was obtained, which was marked as UCN.
[0050] (2) UCN was placed in an open crucible and placed in a muffle furnace for secondary quenching treatment at a heating rate of 20 °C / min, a target temperature of 600 °C, and a holding time of 2 h. Then, it was quenched at room temperature to obtain a white powder sample, which was labeled as PCN.
[0051] (3) 30 mg of PCN was placed in a beaker, 35 mL of ethyl acetate-carbon tetrachloride azeotropic mixture (mass ratio of 43:57) was added, and then 2.0% of ethylene dioleic acid amide surfactant was added, and ultrasonic stirring was performed at an ultrasonic power of 150 W for 12 hours to obtain a uniform mixed suspension;
[0052] (4) The suspension was placed in a reactor for hydrothermal reaction. The volume of the reactor was 50 mL and the material was PPL. The hydrothermal temperature was 180°C and the reaction was kept for 6 hours. After natural cooling, the sample was washed 3 times with water and ethanol respectively and separated by a centrifuge.
[0053] (5) The washed sample was freeze-dried in a vacuum oven and dried thoroughly at a vacuum degree of <15 Pa and a temperature of <-50°C for 24 hours to obtain a white powder sample, which was marked as CCN.
[0054] Example 4
[0055] A method for preparing a hexagonal g-C3N4 (CCN) photocatalyst comprises the following steps:
[0056] (1) 10 g of urea was placed in an alumina crucible and placed in a muffle furnace. The heating rate was set to 5 °C / min, the target temperature was 550 °C, and the holding time was 3 hours. After natural cooling, a light yellow sample was obtained, which was marked as UCN.
[0057] (2) UCN was placed in an open crucible and placed in a muffle furnace for secondary quenching treatment at a heating rate of 20 °C / min, a target temperature of 600 °C, and a holding time of 2 h. Then, it was quenched at room temperature to obtain a white powder sample, which was labeled as PCN.
[0058] (3) 30 mg of PCN was placed in a beaker, 40 mL of ethyl acetate-carbon tetrachloride azeotropic mixture (mass ratio of 43:57) was added, and then 1.5% of ethylene dioleic acid amide surfactant was added, and ultrasonic stirring was performed at an ultrasonic power of 200 W for 2 days to obtain a uniform mixed suspension;
[0059] (4) The suspension was placed in a reactor for hydrothermal reaction. The volume of the reactor was 100 mL and the material was PPL. The hydrothermal temperature was 150° C. and the reactor was kept warm for 12 hours. After natural cooling, the sample was washed three times with water and ethanol respectively and separated by a centrifuge.
[0060] (5) The washed sample was freeze-dried in a vacuum oven and dried thoroughly at a vacuum degree of <15 Pa and a temperature of <-50°C for 24 hours to obtain a white powder sample, which was marked as CCN.
[0061] Example 5
[0062] A method for preparing a hexagonal g-C3N4 (CCN) photocatalyst comprises the following steps:
[0063] (1) 10 g of urea was placed in an alumina crucible and placed in a muffle furnace. The heating rate was set to 5 °C / min, the target temperature was 550 °C, and the holding time was 3 hours. After natural cooling, a light yellow sample was obtained, which was marked as UCN.
[0064] (2) UCN was placed in an open crucible and placed in a muffle furnace for secondary quenching treatment at a heating rate of 20 °C / min, a target temperature of 600 °C, and a holding time of 2 h. Then, it was quenched at room temperature to obtain a white powder sample, which was labeled as PCN.
[0065] (3) 30 mg of PCN was placed in a beaker, 40 mL of ethyl acetate-carbon tetrachloride azeotropic mixture (mass ratio of 43:57) was added, and then 1.5% of ethylene dioleic acid amide surfactant was added, and ultrasonic stirring was performed at an ultrasonic power of 200 W for 2 days to obtain a uniform mixed suspension;
[0066] (4) The suspension was placed in a reactor for hydrothermal reaction. The volume of the reactor was 50 mL and the material was PPL. The hydrothermal temperature was 180°C and the reaction was kept for 6 hours. After natural cooling, the sample was washed 3 times with water and ethanol respectively and separated by a centrifuge.
[0067] (5) The washed sample was freeze-dried in a vacuum oven and dried thoroughly at a vacuum degree of <50 Pa, a temperature of -30°C, and a drying time of 12 hours to obtain a white powder sample, which was marked as CCN.
Claims
1. A method for preparing a hexagonal photocatalyst, characterized in that: The method is prepared by using ultra-thin graphite phase carbon nitride g-C3N4 as raw material, ethyl acetate-carbon tetrachloride azeotropic mixture as solvent, ethylene dioleic acid amide as surfactant, and microwave-assisted recrystallization method. The method for preparing the hexagonal photocatalyst comprises the following steps: (1) Urea is placed in an alumina crucible and placed in a muffle furnace. The heating rate and target temperature are controlled and kept warm for a certain period of time. After natural cooling, a light yellow sample is obtained, which is marked as UCN. (2) UCN was placed in an open crucible and placed in a muffle furnace for secondary quenching to obtain a white powder sample, which was labeled as PCN; (3) placing PCN in a beaker, adding an azeotropic mixture of ethyl acetate and carbon tetrachloride, and then adding an ethylene dioleic acid amide surfactant, and performing high-power ultrasonic stirring to obtain a uniform mixed suspension; (4) placing the suspension into a reactor for hydrothermal reaction, and after natural cooling, washing the sample three times with water and ethanol respectively, and separating the sample using a centrifuge; (5) The washed sample is vacuum freeze-dried to obtain a powdered hexagonal photocatalyst sample, labeled as CCN. The microstructure of the hexagonal photocatalyst is hexagonal with a diameter of 1 to 3 μm, and its surface contains abundant hydroxyl functional groups.
2. The method for preparing the hexagonal photocatalyst according to claim 1, characterized in that: The urea mass of step (1) is 10 g, the heating rate is 5°C / min, the target temperature is 550°C, and the holding time is 3 hours.
3. The method for preparing the hexagonal photocatalyst according to claim 1, characterized in that: The secondary annealing treatment in step (2) has a heating rate of 20°C / min, a target temperature of 600°C, a holding time of 2 hours, and then quenching at room temperature.
4. The method for preparing the hexagonal photocatalyst according to claim 1, characterized in that: The mass ratio of the ethyl acetate-carbon tetrachloride azeotropic mixture in step (3) is 43:57, and the total volume is 40 mL.
5. The method for preparing the hexagonal photocatalyst according to claim 1, characterized in that: The mass fraction of the ethylene dioleic acid amide surfactant in step (3) is 1.5%, the ultrasonic power is 200 W, and the ultrasonic dispersion time is 2 days.
6. The method for preparing the hexagonal photocatalyst according to claim 1, characterized in that: In the hydrothermal reaction of step (4), the volume of the reactor liner is 50 mL, the material is PPL, and the hydrothermal condition is to keep warm at 120-240° C. for 6-12 hours.
7. The method for preparing a hexagonal photocatalyst according to claim 1, characterized in that: The vacuum degree of the vacuum freeze drying in step (5) is <15Pa, the temperature is <-50°C, and the time is 24 hours.
Citation Information
Patent Citations
Preparation method for high specific-surface-area g-C3N4 photocatalyst
CN106552660A
Hexagonal tubular carbon nitride as well as preparation method and application thereof
CN109399584A
Preparation method and application of ultrathin high-crystallinity carbon nitride photocatalyst
CN113318765A
Simple preparation method and application of high-crystallinity graphite carbon nitride
CN114377711A