A nano multiphase jet composite polishing device and method for additively manufacturing the inner wall of a channel heat pipe
Through the nano multi-phase jet composite polishing method, the gas-liquid-solid multi-phase jet is used to accelerate and impact multiple times in a stable flow field, which solves the problems of difficulty in polishing the inner wall of additive manufacturing channel heat pipes and large damage, and achieves more uniform surface removal. and consistent polishing effect.
Patent Information
- Application Number
- CN202211371818.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-11-03
AI Technical Summary
During the polishing process of additively manufactured channel heat pipes, there are problems such as floating powder and slag, traditional polishing methods causing great damage to parts, and poor polishing consistency for thin-walled pipes with large aspect ratios.
The nano multi-phase jet composite polishing method is adopted, and the gas-liquid-solid multi-phase jet nozzle is in sealed contact with the entrance of the heat pipe to form a stable flow field. The atomized small droplets wrap the abrasive particles and accelerate and impact the inner wall multiple times under the action of the high-pressure jet to achieve large-scale polishing. Polishing consistency of the inner wall of the aspect ratio pipe.
It effectively reduces surface impact, improves surface removal uniformity and roughness, reduces polishing damage, and realizes automated processing and dust-free polishing of microstructured slender pipes with simple structure and low maintenance cost.
Smart Images

Figure CN115709439B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of additively manufactured parts polishing, and in particular to a nano multiphase jet composite polishing device and method for the inner wall of an additively manufactured channel heat pipe. Background Art
[0002] Heat pipe is one of the most commonly used heat transfer elements, with high heat transfer coefficient and heat transfer capacity. The grooved heat pipe is a type of heat pipe with stable and reliable operation and wide application. The common groove cross-section area is rectangular and Ω-shaped, and it is usually manufactured by drawing. However, in the direction of spacecraft, in order to reduce weight and reduce processing difficulty, additively manufactured integrated heat pipes have gradually begun to be used. The new grooved heat pipe has an effective length of 200mm, a pipe diameter of 5mm, a wall thickness of 0.8mm, and a groove on the inside of the pipe wall of only 300μm, which is a typical thin-walled groove structure with a large aspect ratio. The use of laser selective melting (SLM) technology to manufacture heat pipes results in a large amount of floating powder and slag attached to the molding surface due to the step effect, powder adhesion, and spheroidization effect. The large size of the slag easily blocks the microchannel of the pipeline, and the floating powder leads to poor surface quality and molding accuracy. The molding accuracy and surface quality of the internal microstructure of the pipeline have a decisive influence on the heat transfer performance. The surface roughness Ra of additively manufactured heat pipes is generally above 10μm. There is a large amount of 100-200μm slag at the bottom of the heat pipe groove, which completely blocks the microstructure and increases the reflux resistance. The surface shape deviation is also above 100μm, resulting in low heat transfer efficiency of the heat pipe.
[0003] Using SLM technology to manufacture heat pipes is a new direction. At the same time, since the new heat pipe is a thin-walled groove structure with a large aspect ratio, the polishing effect of the traditional polishing method is not ideal. For example, there is a significant wall effect in the abrasive flow processing process in the abrasive flow polishing method, which causes differences in the surface roughness and surface morphology of the workpiece and the over-polishing phenomenon at the entrance, resulting in poor consistency of surface quality after processing; abrasive gas jets can perform simple milling and drilling on the surface, but their action depth is generally small, and the removal rate of the heat pipe microchannel structure is large and the erosion effect is serious. In addition to having good inner surface quality, the polishing of the grooved heat pipe should also ensure its corresponding dimensional accuracy, shape accuracy and polishing consistency. Therefore, it is particularly important to develop a suitable polishing method and device for the inner wall of the additively manufactured grooved heat pipe.
[0004] In order to solve the problem of polishing thin-walled grooved pipes with a large aspect ratio, represented by additively manufactured heat pipes, the present invention proposes a nano-multiphase jet composite polishing method and device for the inner wall of an additively manufactured grooved heat pipe. Summary of the invention
[0005] According to the above-mentioned technical problems that a large amount of floating powder and slag exist on the inner wall of the additively manufactured grooved heat pipe, the traditional polishing method causes great damage to the parts, and the polishing consistency of thin-walled pipes with a large aspect ratio is poor, a nano-multiphase jet composite polishing device and method for the inner wall of the additively manufactured grooved heat pipe are provided. The present invention mainly adopts gas-liquid-solid multiphase jet composite polishing. The multiphase jet abrasive is made of aluminum oxide with a diameter of 600#. The multiphase jet nozzle is in sealed contact with the heat pipe inlet through a clamp to prevent pressure loss. A stable flow field is formed inside the narrow heat pipe under the action of the high-pressure jet. Due to the special structure of the heat pipe, a small air compressor can meet the pressure requirement. The atomized small droplets wrap the abrasive and are ejected from the nozzle at a small angle. After the first impact with the inner wall surface of the heat pipe, under the action of the stable flow field, the movement of the abrasive is less affected by air resistance, and will continue to accelerate to a speed close to that of the injection to impact the inner wall surface for the second time. After the second impact, it continues to accelerate under the action of the stable flow field to impact the inner wall surface. The abrasive wrapped in the small droplets is ejected from the heat pipe outlet after multiple accelerations and multiple impacts, thereby achieving the polishing consistency of the inner wall of the pipeline with a large aspect ratio.
[0006] The technical means adopted by the present invention are as follows:
[0007] A nano multiphase jet composite polishing device for the inner wall of an additively manufactured groove heat pipe comprises: an air compressor device, a microcomputer jet control device, a multiphase jet nozzle device, an additively manufactured heat pipe device and a polishing liquid proportioning device, wherein one side of the microcomputer jet control device is connected to the air compressor device, and the other side is connected to one side of the multiphase jet nozzle device; one side of the multiphase jet nozzle device is also connected to the polishing liquid proportioning device, and the other side is sealed with the additively manufactured heat pipe device; the air compressor device is used to provide the entire polishing device with a polishing liquid proportioning device. A high-pressure gas source is provided, and the high-pressure gas is transported to the multiphase jet nozzle device through a microcomputer jet control device; the polishing liquid proportioning device is used to produce a liquid-solid polishing liquid, and transport the polishing liquid to the multiphase jet nozzle device; the multiphase jet nozzle device is used to achieve full mixing and atomization of the liquid-solid polishing liquid and the high-pressure gas to form a gas-liquid-solid multiphase jet, and the gas-liquid-solid multiphase jet is sprayed into the additive manufacturing heat pipe device to perform multiphase jet composite polishing on the workpiece; the microcomputer jet control device is used to adjust the flow of the high-pressure gas and the polishing liquid.
[0008] Furthermore, the polishing liquid is a nano-polishing liquid, which is a mixture of abrasive particles and water, and the abrasive particles are 600-mesh nano-alumina.
[0009] Furthermore, the multiphase jet nozzle device includes an air delivery pipe, a multiphase mixing atomization device, an atomization channel, an atomization nozzle and a gas-liquid interface, one end of the air delivery pipe is connected to the microcomputer jet control device, and the other end is connected to the air inlet end of the gas-liquid interface, and the gas-liquid interface is arranged on one side of the multiphase mixing atomization device; one end of the atomization channel is connected to the other side of the multiphase mixing atomization device, and the other end is connected to the atomization nozzle, and the atomization nozzle is sealed and connected to the additive manufacturing heat pipe device; the multiphase mixing atomization device is also provided with an adjustment switch;
[0010] The gas pipe is used to transport high-pressure gas, and the multiphase mixing atomization device is used to fully mix and atomize the liquid-solid polishing liquid with the high-pressure gas to form a gas-liquid-solid polishing liquid, and then spray the atomized gas-liquid-solid polishing liquid from the atomizing nozzle to the inner surface of the workpiece through the atomization channel.
[0011] Furthermore, the multiphase jet nozzle device also includes a liquid infusion tube, one end of which is connected to the liquid inlet end of the gas-liquid interface, and the other end is connected to the polishing liquid proportioning device; the polishing liquid proportioning device is used to proportion polishing liquids with different abrasive concentrations;
[0012] The polishing liquid proportioning device includes a liquid storage tank, a stirrer and an ultrasonic generator. The liquid storage tank is placed on the ultrasonic generator and is used to contain the polishing liquid. The stirrer includes a bracket and a motor and a stirring blade installed on the bracket. The motor is connected to the stirring blade and is used to drive the stirring blade to rotate and adjust the stirring speed. The lower end of the stirring blade extends into the liquid storage tank and is used to fully stir the polishing liquid. The ultrasonic generator is used to achieve full and uniform dispersion of the abrasive particles in the aqueous solution. The infusion tube extends into the liquid storage tank and is used to transport the polishing liquid that has been stirred to the multiphase mixing atomization device through the gas-liquid interface.
[0013] Furthermore, the additively manufactured heat pipe device is sealed and connected to the atomizing nozzle of the multiphase jet nozzle device through a fixing device and a sealing ring.
[0014] Furthermore, through the impact of high-pressure airflow provided by the air compressor device, the multiphase jet nozzle device breaks the polishing liquid into small droplets to achieve a nano-level atomization effect; the multiphase jet nozzle device adopts a high-pressure resistant flexible liner, both ends of which are sealed by O-rings, and a sleeve-in-tube method is adopted to achieve full sealing of the gas-liquid-solid flow process, forming a stable flow field inside the pipeline.
[0015] Furthermore, the multiphase mixed atomization device atomizes the gas-liquid-solid polishing liquid into abrasive droplets below 10 microns, and under the action of the high-pressure gas, the abrasive droplets are in a floating state in the high-pressure gas. The sprayed atomized polishing liquid has a certain speed but a small impact force. Under the action of the stable flow field formed inside the workpiece, the abrasive droplets scratch and polish the workpiece surface multiple times.
[0016] Furthermore, the connection between the gas-liquid interface and the gas pipe and the liquid infusion tube is sealed and fixed by a sealing ring; the ends of the gas pipe and the liquid infusion tube connected to the gas-liquid interface are both quick-connect connectors to achieve a tight connection.
[0017] The present invention also provides a polishing method of a nano multiphase jet composite polishing device for additively manufacturing the inner wall of a channel heat pipe, comprising the following steps:
[0018] Step 1: sealing and fixing the atomizing nozzle and the heat pipe additive manufacturing heat pipe device through a fixing device and a sealing ring;
[0019] Step 2: Start the polishing liquid proportioning device, prepare the polishing liquid with the required abrasive concentration, use the stirring blade to fully stir the abrasive and the aqueous solution, and after the stirring is completed, transport the polishing liquid through the gas-liquid interface to the multiphase mixing atomization device of the multiphase jet nozzle device through the infusion tube, and adjust the flow rate of the polishing liquid through the regulating switch;
[0020] Step three, start the air compressor device, and transport the high-pressure gas to the multi-phase mixed atomization device through the air pipe and the microcomputer intelligent controller. In the multi-phase mixed atomization device, the gas, liquid and abrasive are fully mixed and atomized to form a gas-liquid-solid polishing liquid, and the gas-liquid-solid polishing liquid is transported to the atomizing nozzle through the atomizing channel in the form of a gas-liquid-solid multi-phase jet under high pressure, and then sprayed to the additive manufacturing heat pipe device at a small angle through the atomizing nozzle to perform gas-liquid-solid three-phase composite polishing on the surface of the workpiece; in this process, the microcomputer jet control device is used to adjust the amount of high-pressure gas passing through, and the working time can also be set. After the set time is reached, the polishing process automatically stops to meet the needs of automated polishing.
[0021] Furthermore, in the step 3, under the action of the high-pressure jet, a stable flow field is formed inside the workpiece, and the gas-liquid-solid polishing liquid formed after mixed atomization presents atomized small droplets wrapping the abrasive particles, which are ejected from the atomizing nozzle at a small angle;
[0022] The ejected abrasive particles are wrapped with a layer of liquid film. After the abrasive particles wrapped by the liquid film impact with the inner wall surface of the workpiece for the first time, under the action of the stable flow field, the movement of the abrasive particles is less affected by the air resistance, and will continue to accelerate to a speed close to that at the time of injection and impact with the inner wall surface for the second time. After the second impact, they continue to accelerate under the action of the stable flow field and impact with the inner wall surface. The abrasive particles wrapped by the liquid film are ejected from the workpiece outlet after multiple accelerations and multiple impacts, thereby achieving the polishing consistency of the inner wall of the pipeline with a large aspect ratio. Among them, the stable flow field provides energy and acceleration for the abrasive particles multiple times, thereby realizing a cycle of acceleration-impact-acceleration of the abrasive particles inside the workpiece.
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] 1. The nano multiphase jet composite polishing device and method for the inner wall of the additively manufactured grooved heat pipe provided by the present invention, compared with the traditional polishing method, the abrasive particles are wrapped in liquid, and the buffering effect of the water film and the static pressure of the liquid water hammer when colliding with the surface can effectively reduce the impact on the surface, and achieve more uniform surface removal and better surface roughness under the same abrasive particle size.
[0025] 2. The nano multiphase jet composite polishing device and method for the inner wall of the additively manufactured groove heat pipe provided by the present invention, the nozzle and the heat pipe in the multiphase jet device are sealed and fixedly connected by a fixing device and a sealing ring, reducing the pressure loss at the inlet of the heat pipe, forming a stable flow field inside the heat pipe, and the abrasive droplets will continue to accelerate in the flow field after colliding with the workpiece inside the heat pipe, and then collide with the surface to continue material removal. However, the pressure of the general sandblasting and spraying methods is completely lost at the nozzle outlet, and the abrasive particles and droplets are severely decelerated by the external air resistance, and the number of secondary collisions is reduced.
[0026] 3. The nano multiphase jet composite polishing device and method for the inner wall of the additively manufactured grooved heat pipe provided by the present invention has the characteristic of contour polishing along the inner wall. The abrasive flow is in close contact with the inner wall, and the abrasive particles scratch the surface contour of the inner wall. The floating powder and slag after polishing are carried away by the turbulent flow of the flowing viscous abrasive particles, which can realize the automated and flexible processing of microstructured slender pipes.
[0027] 4. The nano multiphase jet composite polishing device and method for the inner wall of the additively manufactured groove heat pipe provided by the present invention has the advantage of dust-free polishing. Since the droplets sprayed out quickly condense and settle, the polishing abrasive particles will not cause dust hazards.
[0028] 5. The nano multiphase jet composite polishing device and method for the inner wall of the additively manufactured groove heat pipe provided by the present invention has a simple structure, low operation and maintenance cost, and high stability, and an air compressor can meet the air pressure requirements of the device.
[0029] In summary, the application of the technical solution of the present invention can solve the problems of difficulty in polishing the inner wall of thin-walled groove pipes with a large aspect ratio, represented by additively manufactured heat pipes, large polishing damage and polishing consistency.
[0030] Based on the above reasons, the present invention can be widely promoted in the fields of polishing and the like. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0032] Figure 1 It is a schematic diagram of the structure of the nano multiphase jet composite polishing device of the present invention.
[0033] Figure 2 Schematic diagram of the cross-sectional structure of an additively manufactured heat pipe of the present invention, wherein (a) is one additively manufactured heat pipe, and (b) is another additively manufactured heat pipe.
[0034] Figure 3 The figures are the polishing effect diagrams of the inner wall of the pipeline before polishing, the traditional polishing method and the multiphase jet composite polishing method under stable polishing time, wherein (a) is a schematic diagram of the inner wall of the pipeline before polishing, (b) is a polishing effect diagram of the inner wall of the pipeline obtained by the traditional polishing method, and (c) is a polishing effect diagram of the inner wall of the pipeline obtained by the multiphase jet composite polishing method.
[0035] In the figure: 1. Air compressor; 2. Microcomputer intelligent controller; 3-1. Air pipe; 3-2. Adjustment switch; 3-3. Multiphase mixing atomization device; 3-4. Atomization channel; 3-5. Atomization nozzle; 3-6. Fixing device; 3-7. Gas-liquid interface; 3-8. Liquid infusion pipe; 4. Additive manufacturing heat pipe device; 5-1. Liquid storage tank; 5-2. Ultrasonic generator; 5-3. Stirring blade. DETAILED DESCRIPTION
[0036] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0037] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0039] Unless otherwise specifically stated, the relative arrangement, numerical expressions and numerical values of the parts and steps described in these embodiments do not limit the scope of the present invention. At the same time, it should be clear that, for ease of description, the sizes of the various parts shown in the drawings are not drawn according to the actual proportional relationship. The technology, methods and equipment known to ordinary technicians in the relevant field may not be discussed in detail, but in appropriate cases, the technology, methods and equipment should be regarded as a part of the authorization specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.
[0040] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "lateral, vertical, perpendicular, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the drawings. They are only for the convenience of describing the present invention and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the device or element referred to must have a specific direction or be constructed and operated in a specific direction. Therefore, they cannot be understood as limiting the scope of protection of the present invention: the directional words "inside and outside" refer to the inside and outside relative to the contours of each component itself.
[0041] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below their position devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.
[0042] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.
[0043] In order to overcome the shortcomings of the prior art, the present invention proposes a nano-multiphase jet composite polishing method for the inner wall of an additively manufactured grooved heat pipe, in view of the problems of a large amount of floating powder and slag on the inner wall of the additively manufactured grooved heat pipe, the serious damage to parts caused by traditional polishing methods, and the poor polishing consistency of thin-walled pipes with a large aspect ratio. The method adopts gas-liquid-solid multiphase jet composite polishing. The multiphase jet abrasive is made of 600# diameter aluminum oxide. The multiphase jet nozzle (i.e., atomizing nozzle) is sealed and contacted with the heat pipe inlet through a clamp (i.e., fixing device) to prevent pressure loss. A stable flow field is formed inside the narrow heat pipe under the action of high-pressure jet. Due to the special structure of the heat pipe, a small air compressor can meet the pressure requirement. The atomized small droplets are wrapped with the abrasive and ejected from the nozzle at a small angle. After the first impact with the inner wall surface of the heat pipe, under the action of the stable flow field, the movement of the abrasive is less affected by air resistance and will continue to accelerate to a speed close to that of the injection to impact the inner wall surface for the second time. After the second impact, it continues to accelerate under the action of the stable flow field to impact the inner wall surface. The abrasive wrapped in the small droplets is ejected from the heat pipe outlet after multiple accelerations and multiple impacts, thereby achieving the polishing consistency of the inner wall of the pipeline with a large aspect ratio.
[0044] When polishing parts with traditional abrasive gas jets, the abrasive particles will quickly release pressure after leaving the nozzle. At the same time, the movement of the abrasive particles is also affected by air resistance, resulting in an effective polishing distance of only about 50 mm, and the polishing effect decreases with the increase of the polishing distance. With the further increase in demand, the current heat pipe length can reach more than 200 mm, while the pipe diameter is only 5 mm, and the pipe aspect ratio is 40:1. Therefore, the traditional abrasive gas jet polishing method is difficult to meet the polishing requirements of thin-walled channel pipes with large aspect ratios represented by additively manufactured heat pipes. The nano-multiphase jet composite polishing method of the present invention seals the nozzle with the heat pipe inlet, and the high-pressure airflow forms a stable flow field during the circulation inside the narrow heat pipe, and the air resistance and pressure loss in the stable flow field are small. The stable flow field can provide energy and acceleration for the abrasive particles multiple times, realizing the cycle of acceleration-impact-acceleration of the abrasive particles inside the pipeline, greatly increasing the polishing distance of the abrasive particles. The stable polishing distance can reach more than 400 mm, which is about 8 times the traditional polishing distance. At the same time, due to the existence of the stable flow field, the speed of the abrasive particles after each acceleration is almost the same as the speed at the time of injection, and the polishing effect at the pipeline outlet is close to that at the inlet, which effectively alleviates the problem that the polishing effect decreases with the increase of the polishing distance in the traditional polishing method. The multiphase jet composite polishing method significantly improves the polishing consistency of large aspect ratio groove pipelines such as heat pipes.
[0045] The abrasive particles in the traditional abrasive air jet polishing method directly impact the inner surface of the pipe, resulting in obvious plastic scratches and poor inner surface roughness. The water pressure of the traditional abrasive water jet polishing method is tens to hundreds of MPa, and the abrasive is ejected at a high speed of hundreds of meters per second. This method will cause a devastating impact on the microchannel structure inside the heat pipe.
[0046] The nano multiphase jet composite polishing method of the present invention adopts gas-liquid-solid three-phase mixed polishing. The abrasive particles ejected from the nozzle are coated with a layer of liquid film. The gas pressure is small and the abrasive particles ejected from the multiphase jet under the same gas pressure have a lower speed. A layer of water film will be formed on the inner surface of the pipe wall. When the abrasive particles wrapped in the liquid film collide with the inner surface of the pipe wall, the static pressure of the water hammer plays a buffering effect. The multiphase jet composite polishing method effectively reduces the plastic removal depth of the material, improves the surface roughness, and ensures the service life of the pipeline as well as the size and shape accuracy.
[0047] The novelty of the method of the present invention compared with the traditional polishing method:
[0048] (1) Compared with traditional polishing methods, the abrasive particles in multiphase jet are wrapped in liquid. When they collide with the surface, the buffering effect of the water film and the static pressure of the liquid water hammer can effectively reduce the impact on the surface, achieving more uniform surface removal and better surface roughness under the same abrasive particle size.
[0049] (2) The nozzle and heat pipe in the multiphase jet device are sealed and fixedly connected through a fixing device and a sealing ring, which reduces the pressure loss at the heat pipe inlet and forms a stable flow field inside the heat pipe. After the abrasive droplets collide with the workpiece once inside the heat pipe, they will continue to accelerate in the flow field and then collide with the surface to continue material removal. In general sandblasting and spraying methods, the pressure is completely lost at the nozzle outlet, and the abrasive and droplets are severely decelerated by the external air resistance, and the number of secondary collisions is reduced.
[0050] (3) The multiphase jet has the characteristic of polishing along the inner wall. The abrasive flow is in close contact with the inner wall, and the abrasive particles scratch the surface contour of the inner wall. The floating powder and slag after polishing are carried away by the turbulent flow of the flowing viscous abrasive particles, which can realize the automated and flexible processing of microstructured slender pipes.
[0051] (4) Multiphase jet has the advantage of dust-free polishing. Since the liquid droplets sprayed out quickly condense and settle, the polishing abrasive particles will not cause dust hazards.
[0052] (5) The multiphase jet polishing device has a simple structure, low operating and maintenance costs, and high stability. The air compressor can meet the air pressure requirements of the device.
[0053] The present invention provides a nano multiphase jet composite polishing device for the inner wall of an additively manufactured groove heat pipe, comprising: a microcomputer jet control device, a multiphase jet nozzle device, a polishing liquid proportioning device, an additively manufactured heat pipe device and an air compressor device. The multiphase jet nozzle device is used to fully mix gas, liquid and abrasive particles, and can adjust the amount of polishing liquid entering. On the other hand, the device sprays the polishing liquid at a small angle to the inner surface of the heat pipe through a nozzle under high pressure; the microcomputer jet control device can accurately control and adjust the amount of high-pressure gas passing through; the air compressor device provides high-pressure airflow for the entire device; the polishing liquid proportioning device is used to proportion polishing liquids with different abrasive concentrations, and enter the multiphase jet nozzle device through a liquid infusion tube.
[0054] In this embodiment, the microcomputer jet control device can be adjusted intelligently to effectively control the air pressure flowability. The microcomputer jet control device can set the working time, and the polishing process automatically stops after the set time is reached, meeting the needs of automated polishing.
[0055] In this embodiment, the multiphase jet nozzle device is the gas-liquid-solid mixing end and output end of the nano-multiphase jet composite polishing device. The device breaks the polishing liquid into small droplets under the impact of the high-pressure airflow provided by the air compressor, thereby achieving a nano-level atomization effect. The multiphase jet nozzle device adopts a high-pressure resistant flexible liner, which is sealed by O-rings at both ends. In addition, a sleeve-in-tube method is adopted to achieve full sealing of the gas-liquid-solid flow process, forming a stable flow field inside the pipeline. The advantage of this device is that the atomization effect is very good, the pressure requirement is not high, and it is suitable for polishing slender pipeline precision parts.
[0056] In this embodiment, the other end of the multiphase jet nozzle device is a gas-liquid-solid multiphase jet mixing device, including a Y-shaped and internally connected joint pipeline, one end of the two Y-shaped channels of the joint pipeline is a liquid-solid end, and the other end is an air inlet end. The gas-liquid-solid mixture flowing out of one side of the single channel is called the mixing end. The air pressure is set to 0.6MPa, and the polishing liquid automatically flows into the multiphase jet nozzle device under the action of the air pressure. The solid-liquid and air inlet pipelines are 8mm quick-plug connectors, which can achieve a tight connection with the joint pipeline. Through the Y-shaped structure of the joint pipeline, after the gas and polishing liquid are introduced at the same time, since the mixing piece passing through is a porous structure, the pores can produce tiny bubbles, so that the effect of uniform mixing of gas, liquid and solid phases can be achieved at the mixing end, thereby meeting the polishing requirements.
[0057] In this embodiment, the air compressor is used as the high-pressure air source of the nano multiphase jet composite polishing device, which atomizes the polishing liquid into micron droplets after high-speed impact in the device, pushes the droplets to be ejected at the nozzle of the multiphase jet nozzle, and forms a stable flow field inside the additive manufacturing heat pipe device. Since the polishing pipe has a small diameter and the outlet channel has a small diameter, the air compressor can meet the demand.
[0058] In this embodiment, the polishing liquid proportioning device provides nano-polishing liquid for the nano-multiphase jet composite polishing device. Pure water is selected as the carrier of the polishing abrasive particles, and 600 mesh nano-alumina is used as the abrasive particles. However, the nano-abrasive particles are not easy to fully suspend in the aqueous solution, which will lead to problems such as uneven polishing and blocked channels. A polishing liquid proportioning device is designed to meet the requirements of adding an appropriate amount of water and nano-abrasive particles to the polishing liquid proportioning device and modulating them according to a certain content to obtain a nano-polishing liquid with water as the carrier and uniform distribution of abrasive particles.
[0059] In this embodiment, the polishing liquid proportioning device includes a liquid storage tank, a small laboratory mixer and an ultrasonic generator. In order to make the abrasive particles in the obtained nano-polishing liquid evenly distributed, the mixer is required to fully stir the polishing liquid before and during polishing. The mixer is suitable for mixing and stirring low and medium viscosity liquids in laboratories or outdoor experiments. The materials in the mixer have axial movement and circular movement at the same time, so there are several stirring forms such as shear stirring and diffusion stirring at the same time, which can make the nano-abrasive particles evenly distributed in the polishing liquid. However, it is still difficult for the existing small stirring device to achieve complete and uniform dispersion of nano-abrasive particles in aqueous solution. Therefore, it is further proposed to use ultrasonic technology to assist in achieving full and uniform dispersion of abrasive particles in aqueous solution. The ultrasonic generator combined with a small mixer can effectively achieve uniform dispersion of nano-abrasive particles in aqueous solution. The device can effectively solve the problem that abrasive particles in nano multiphase jet composite polishing are difficult to evenly disperse in aqueous solution.
[0060] By comparing the method and device of the present invention with the existing methods and devices, it is concluded that the method of the present invention forms a stable flow field inside the heat pipe, and the abrasive particles can accelerate the scratching and removal of surface floating powder and slag multiple times. Due to the presence of water film coating the abrasive particles, the polishing surface accuracy is high, and the polishing consistency effect of the slender heat pipe is significant. There is no obvious wear and scratches on the inner wall of the heat pipe, and the polishing effect is significant and stable.
[0061] The present invention also provides a polishing method of a nano multiphase jet composite polishing device for additively manufacturing the inner wall of a channel heat pipe, comprising the following steps:
[0062] Step 1: sealing and fixing the atomizing nozzle and the heat pipe additive manufacturing heat pipe device through a fixing device and a sealing ring;
[0063] Step 2: Start the polishing liquid proportioning device, prepare the polishing liquid with the required abrasive concentration, use the stirring blade to fully stir the abrasive and the aqueous solution, and after the stirring is completed, transport the polishing liquid through the gas-liquid interface to the multiphase mixing atomization device of the multiphase jet nozzle device through the infusion tube, and adjust the flow rate of the polishing liquid through the regulating switch;
[0064] Step three, start the air compressor device, and transport the high-pressure gas to the multi-phase mixed atomization device through the air pipe and the microcomputer intelligent controller. In the multi-phase mixed atomization device, the gas, liquid and abrasive are fully mixed and atomized to form a gas-liquid-solid polishing liquid, and the gas-liquid-solid polishing liquid is transported to the atomizing nozzle through the atomizing channel in the form of a gas-liquid-solid multi-phase jet under high pressure, and then sprayed to the additive manufacturing heat pipe device at a small angle through the atomizing nozzle to perform gas-liquid-solid three-phase composite polishing on the surface of the workpiece; in this process, the microcomputer jet control device is used to adjust the amount of high-pressure gas passing through, and the working time can also be set. After the set time is reached, the polishing process automatically stops to meet the needs of automated polishing.
[0065] Example 1
[0066] like Figure 1 As shown, the nano multiphase jet composite polishing device of the present invention includes an air compressor device (selecting air compressor 1), a microcomputer jet control device (selecting microcomputer intelligent controller 2), a multiphase jet nozzle device, an additive manufacturing heat pipe device 4 and a polishing liquid proportioning device. The multiphase jet nozzle device includes an air delivery pipe 3-1, a multiphase mixing atomization device 3-3, an atomization channel 3-4, an atomization nozzle 3-5, a gas-liquid interface 3-7 and a liquid delivery pipe 3-8. The polishing liquid proportioning device includes a liquid storage tank 5-1, a stirrer and an ultrasonic generator 5-2, and the stirrer includes a bracket, a motor and a stirring blade 5-3.
[0067] The air compressor device provides a high-pressure gas source for the entire polishing device, and transmits the high-pressure gas to the microcomputer intelligent controller 2 through the gas pipe 3-1; one end of the microcomputer intelligent controller 2 is connected to the air compressor device, and the other end is connected to the multiphase jet nozzle device through the gas pipe 3-1, which has a regulating effect on the flow of high-pressure gas and polishing liquid; the multiphase jet nozzle device fully mixes and atomizes the liquid-solid polishing liquid and the high-pressure gas in the multiphase mixing atomization device 3-3, and then sprays the abrasive polishing liquid to the additive manufacturing heat pipe device through the main pipeline (atomization channel 3-4) and nozzle (atomization nozzle 3-5) of the device; the polishing liquid proportioning device drives the stirring blade 5-3 to rotate through the motor, fully mixes the nano-abrasive and the aqueous solution to form a polishing liquid, and then transports it to the multiphase jet nozzle device through the infusion pipe 3-8.
[0068] In this embodiment, the microcomputer jet control device can effectively adjust the gas flow rate of the air compressor device.
[0069] In this embodiment, the gas-liquid interface 3-7 in the multiphase jet nozzle device is respectively connected to the gas pipe 3-1 and the liquid pipe 3-8, and the connection points are sealed and fixed with sealing rings. At the same time, the gas-liquid-solid flowability is good. The ends of the gas pipe 3-1 and the liquid pipe 3-8 connected to the gas-liquid interface 3-7 are quick-plug connectors to achieve a tight connection; the gas pipe 3-1 connects the microcomputer intelligent controller 2 and the atomizing nozzle 3-5, and the liquid pipe 3-8 connects the polishing liquid proportioning device and the atomizing nozzle 3-5, and the connection method has good airtightness; the multiphase jet nozzle device atomizes the polishing liquid into abrasive droplets below 10 microns, and under the action of high-pressure gas, it is in a floating state in the high-pressure gas. The sprayed atomized polishing liquid has a certain speed but a small impact force. Under the action of the stable flow field formed inside the heat pipe, the abrasive droplets scratch and polish the surface of the workpiece many times. The multiphase jet nozzle device is also provided with an adjustment switch 3-2, which is connected to the microcomputer intelligent controller and is used to adjust the flow rate of the polishing liquid delivered to the multiphase jet nozzle device.
[0070] In this embodiment, the additive manufacturing heat pipe device 4 is connected to the atomizing nozzle 3-5 of the multiphase jet nozzle device through the fixing device 3-6 and the sealing ring, and has good air tightness and stability. Figure 2 Shown are schematic structural diagrams of two additively manufactured heat pipes (workpieces to be processed) in this embodiment.
[0071] In this embodiment, the support of the stirrer in the polishing liquid proportioning device is used to fix the driving motor and the stirring blade 5-3. The driving motor can adjust the stirring speed of the stirring blade 5-3. The stirring blade 5-3 fully stirs the nano-polishing liquid. The polishing liquid is stored in the liquid storage tank 5-1. The liquid storage tank 5-1 is placed on the ultrasonic generator 5-2, and the nano-abrasive particles are further evenly distributed in the aqueous solution by ultrasonic assistance. The lower end of the infusion tube 3-8 extends into the liquid storage tank 5-1, and the polishing liquid after stirring is transported to the multi-phase mixing atomization device 3-3 through the gas-liquid interface 3-7.
[0072] In this embodiment, aluminum oxide nano-abrasive with a mesh size of 600 was selected, and polishing liquids with abrasive contents of 0, 0-5%, 5-10%, 10-15%, 15-20%, and 20-25% were respectively prepared to investigate the polishing effect. The air pressure was set to 0.6 MPa, and the polishing time was 15 minutes. The specific parameters are shown in the following table.
[0073]
[0074] In this embodiment, the polishing nozzle is stably and tightly connected to the heat pipe, the polishing liquid proportioning device is started first, and then the air compressor device is started to start polishing. After the polishing is completed, the macroscopic morphology of the inner surface of the pipeline microchannel is observed by electron microscope.
[0075] The results show that when the abrasive content is 0, the inner wall of the microchannel is a material layer formed by the step effect, and a large amount of slag blocks the channel, a large amount of molten floating powder adheres to the surface, and the quality of the inner surface of the pipeline is very poor; when the polishing abrasive content is 0-5%, the abrasive washes away the loose large-particle slag in the inner wall of the microchannel, and at the same time, the abrasive in the polishing droplets performs preliminary micro-cutting on the protruding material layer, so that the surface protrusions are purified. When the polishing abrasive content is 5-10%, the smoothness of the inner wall of the microchannel is improved compared with the abrasive content of 0-5%, but it can still be observed that relatively small particles of floating powder and slag are attached to the inner wall of the pipe; when the abrasive content reaches 5-10% and 10-15%, the surface quality of the inner wall of the microchannel is further improved; when the abrasive content reaches 15-20%, the inner wall of the microchannel presents a better surface quality as a whole, the shape accuracy is improved, the slag at the bottom of the groove is completely removed, and the surface is basically flattened; when the abrasive content reaches 20-25%, the roughness value of the inner wall of the microchannel does not change much, but there are fine abrasive diversion marks on the inner surface of the pipe wall, and obvious scratch tracks are formed on the surface, which does not meet the requirements of high-quality polishing. Therefore, the polishing effect of the inner wall of the microchannel is different under different polishing abrasive contents. Within the same polishing time, the polishing effect of the inner wall surface of the microchannel first increases and then decreases with the increase of the abrasive content, and it is more reasonable when the abrasive content is 15-20%.
[0076] The polishing effects of the multiphase jet polishing method and the traditional polishing method were verified by comparing the experimental device. The experiment selected abrasives of the same mesh size and material and configured with the same concentration of polishing liquid. The polishing experiment was carried out on the same batch of additively manufactured large aspect ratio groove heat pipes. The results were analyzed based on the surface roughness of the inner wall of the heat pipe and the structural size deviation.
[0077] In this embodiment, the polishing effects of the conventional abrasive gas jet polishing method and the multiphase jet composite polishing method are compared under the premise of the same abrasive content and abrasive mesh size. Figure 3 Shown are the polishing effects of the inner wall of the pipeline before polishing, under the stable polishing time of the traditional polishing method and the multiphase jet composite polishing method.
[0078] The results show that when the stable polishing state is reached, the roughness of the inner surface of the polished pipe by the traditional polishing method decreases from 15μm before polishing to 6μm, and the roughness of the inner surface of the polished pipe by the multiphase jet composite polishing method decreases from 15μm before polishing to 3μm, which is about doubled compared with the traditional polishing method; the deviation of the internal bottom structure size of the polished pipe by the multiphase jet composite polishing method decreases by 30μm, and the deviation of the internal bottom structure size of the polished pipe by the traditional polishing method decreases by 90μm. The material removal is three times that of the new method, which destroys the microchannel structure inside the pipe and causes serious over-polishing. In addition, since the abrasive particles move relatively stably inside the pipe in the multiphase jet composite polishing method, the material removal of the abrasive particles on the inner wall groove of the pipe is relatively balanced, and the polishing effects at the inlet and outlet of the pipe are similar, achieving a consistent polishing effect. This proposes an effective method and device for the polishing problem of the inner wall of the thin-walled groove pipe with a large aspect ratio, represented by the additive manufacturing heat pipe.
[0079] In summary, the method and device of the present invention have a significant effect on improving the surface quality of the inner wall of the additively manufactured rectangular and Ω-shaped groove heat pipes, without destroying the dimensional accuracy of the heat pipe structure, and the polishing consistency effect is obvious, which can achieve the expected goal.
[0080] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A nano multiphase jet composite polishing device for additive manufacturing of the inner wall of a channel heat pipe, characterized in that: include: An air compressor device, a microcomputer jet control device, a multiphase jet nozzle device, an additive manufacturing heat pipe device (4) and a polishing liquid proportioning device, wherein one side of the microcomputer jet control device is connected to the air compressor device, and the other side is connected to one side of the multiphase jet nozzle device; one side of the multiphase jet nozzle device is also connected to the polishing liquid proportioning device, and the other side is sealedly connected to the additive manufacturing heat pipe device (4); the air compressor device is used to provide a high-pressure gas source for the entire polishing device, and to transport the high-pressure gas to the multiphase jet nozzle device through the microcomputer jet control device; the polishing liquid proportioning device is used to generate liquid-solid polishing liquid, and to transport the polishing liquid to the multiphase jet nozzle device; the multiphase jet nozzle device is used to achieve full mixing and atomization of the liquid-solid polishing liquid and the high-pressure gas to form a gas-liquid-solid multiphase jet, and to spray the gas-liquid-solid multiphase jet into the additive manufacturing heat pipe device (4) to perform multiphase jet composite polishing on the workpiece; the microcomputer jet control device is used to adjust the flow of the high-pressure gas and the polishing liquid; The multiphase jet nozzle device comprises an air delivery pipe (3-1), a multiphase mixing atomization device (3-3), an atomization channel (3-4), an atomization nozzle (3-5) and a gas-liquid interface (3-7); one end of the air delivery pipe (3-1) is connected to a microcomputer jet control device, and the other end is connected to an air inlet end of the gas-liquid interface (3-7); the gas-liquid interface (3-7) is arranged on one side of the multiphase mixing atomization device (3-3); one end of the atomization channel (3-4) is connected to the other side of the multiphase mixing atomization device (3-3), and the other end is connected to the atomization nozzle (3-5); the atomization nozzle (3-5) is sealedly connected to the additive manufacturing heat pipe device (4); the multiphase mixing atomization device (3-3) is also provided with an adjustment switch (3-2); The gas delivery pipe (3-1) is used to realize the delivery of high-pressure gas, and the multiphase mixing atomization device (3-3) is used to fully mix the liquid-solid polishing liquid with the high-pressure gas to form a gas-liquid-solid polishing liquid, and the atomized gas-liquid-solid polishing liquid is sprayed from the atomization nozzle (3-5) to the inner surface of the workpiece through the atomization channel (3-4).
2. The nano multiphase jet composite polishing device for the inner wall of the additively manufactured groove heat pipe according to claim 1, characterized in that: The polishing liquid is a nano polishing liquid, which is formed by mixing abrasive grains and water, and the abrasive grains are 600-mesh nano aluminum oxide.
3. The nano multiphase jet composite polishing device for additively manufacturing the inner wall of a channel heat pipe according to claim 1, characterized in that: The multiphase jet nozzle device also includes a liquid infusion tube (3-8), one end of which is connected to the liquid inlet end of the gas-liquid interface (3-7), and the other end of which is connected to a polishing liquid proportioning device; the polishing liquid proportioning device is used to proportion polishing liquids with different abrasive concentrations; The polishing liquid proportioning device comprises a liquid storage tank (5-1), a stirrer and an ultrasonic generator (5-2); the liquid storage tank (5-1) is placed on the ultrasonic generator (5-2) and is used to contain the polishing liquid; the stirrer comprises a bracket and a motor and a stirring blade (5-3) mounted on the bracket; the motor is connected to the stirring blade (5-3) and is used to drive the stirring blade (5-3) to rotate and adjust the stirring speed; the lower end of the stirring blade (5-3) extends into the liquid storage tank (5-1) and is used to fully stir the polishing liquid; the ultrasonic generator (5-2) is used to achieve full and uniform dispersion of abrasive particles in the aqueous solution; the infusion tube (3-8) extends into the liquid storage tank (5-1) and is used to transport the polishing liquid that has been stirred to the multiphase mixing atomization device (3-3) through the gas-liquid interface (3-7).
4. The nano multiphase jet composite polishing device for additively manufacturing the inner wall of a grooved heat pipe according to claim 1 or 2, characterized in that: The additively manufactured heat pipe device (4) is sealed and connected to the atomizing nozzle (3-5) of the multi-phase jet nozzle device via a fixing device (3-6) and a sealing ring.
5. The nano multiphase jet composite polishing device for additively manufacturing the inner wall of a grooved heat pipe according to claim 4, characterized in that: The multiphase jet nozzle device breaks the polishing liquid into small droplets through the impact of high-pressure airflow provided by the air compressor device, thereby achieving a nano-level atomization effect; the multiphase jet nozzle device adopts a high-pressure resistant flexible liner, both ends of which are sealed by O-rings, and a sleeve-in-tube method is adopted to achieve full sealing of the gas-liquid-solid flow process, thereby forming a stable flow field inside the pipeline.
6. The nano multiphase jet composite polishing device for additively manufacturing the inner wall of a channel heat pipe according to claim 5, characterized in that: The multiphase mixed atomization device (3-3) atomizes the gas-liquid-solid polishing liquid into abrasive droplets of less than 10 microns, and under the action of the high-pressure gas, the abrasive droplets are in a floating state in the high-pressure gas. The sprayed atomized polishing liquid has a certain speed but a small impact force. Under the action of the stable flow field formed inside the workpiece, the abrasive droplets scratch and polish the surface of the workpiece multiple times.
7. The nano multiphase jet composite polishing device for additively manufacturing the inner wall of a channel heat pipe according to claim 3, characterized in that: The connection points between the gas-liquid interface (3-7) and the gas pipe (3-1) and the liquid pipe (3-8) are sealed and fixed by sealing rings; the ends of the gas pipe (3-1) and the liquid pipe (3-8) connected to the gas-liquid interface (3-7) are both quick-connect connectors to achieve a tight connection.
8. A polishing method for the inner wall of a grooved heat pipe manufactured by an additively manufactured nano multiphase jet composite polishing device as claimed in any one of claims 1 to 7, characterized in that: The steps include: Step 1: sealing and fixing the atomizing nozzle (3-5) and the heat pipe additive manufacturing heat pipe device (4) through a fixing device (3-6) and a sealing ring; Step 2: Start the polishing liquid proportioning device, prepare the polishing liquid with the required abrasive concentration, use the stirring blade (5-3) to fully stir the abrasive and the aqueous solution, and after the stirring is completed, transport the polishing liquid through the infusion pipe (3-8) and the gas-liquid interface (3-7) to the multiphase mixing atomization device (3-3) of the multiphase jet nozzle device, and adjust the flow rate of the polishing liquid by adjusting the switch (3-2); Step 3, start the air compressor device, and deliver the high-pressure gas to the multi-phase mixed atomization device (3-3) through the gas delivery pipe (3-1) and the microcomputer intelligent controller. In the multi-phase mixed atomization device (3-3), the gas, liquid and abrasive are fully mixed and atomized to form a gas-liquid-solid polishing liquid, and the gas-liquid-solid polishing liquid is delivered to the atomizing nozzle (3-5) through the atomizing channel (3-4) in the form of a gas-liquid-solid multi-phase jet under the action of high pressure, and is sprayed at a small angle to the additive manufacturing heat pipe device (4) through the atomizing nozzle (3-5) to perform gas-liquid-solid three-phase composite polishing on the surface of the workpiece; in this process, the high-pressure gas flow rate is adjusted by the microcomputer jet control device, and the working time can also be set. After the set time is reached, the polishing process automatically stops to meet the needs of automated polishing.
9. The polishing method of the nano multiphase jet composite polishing device for the inner wall of the additively manufactured grooved heat pipe according to claim 8, characterized in that: In the step 3, under the action of the high-pressure jet, a stable flow field is formed inside the workpiece, and the gas-liquid-solid polishing liquid formed after mixed atomization presents atomized small droplets wrapping the abrasive particles, which are ejected from the atomizing nozzle at a small angle; The ejected abrasive particles are wrapped with a layer of liquid film. After the abrasive particles wrapped by the liquid film impact with the inner wall surface of the workpiece for the first time, under the action of the stable flow field, the movement of the abrasive particles is less affected by the air resistance, and will continue to accelerate to a speed close to that at the time of injection and impact with the inner wall surface for the second time. After the second impact, they continue to accelerate under the action of the stable flow field and impact with the inner wall surface. The abrasive particles wrapped by the liquid film are ejected from the workpiece outlet after multiple accelerations and multiple impacts, thereby achieving the polishing consistency of the inner wall of the pipeline with a large aspect ratio. Among them, the stable flow field provides energy and acceleration for the abrasive particles multiple times, thereby realizing a cycle of acceleration-impact-acceleration of the abrasive particles inside the workpiece.
Citation Information
Patent Citations
Device and method for processing surface texture through micro-abrasive multiphase jetting
CN105234824A
Device for assisting electrolytic machining of micro-grooves through abrasive jet based on gas driving
CN107649839A
Ultrasonic cavitation assistant jet polishing system and polishing method
CN110026908A
Spraying apparatus and cleaning device
WO2020094053A1
Cited By
Immersion type automatic polishing equipment for complex curved surface part
CN120002539A
Cavitation enhanced multiphase jet corrosion auxiliary polishing device and method for additive manufacturing complex inner runner
CN121777054A