Neutral leaching method and system for uranium
By utilizing the chemical reaction of carbon dioxide and limestone in the reaction tower and soaking tank, the bicarbonate concentration in the neutral ground uranium leaching process is increased, and the problem of low HCO3- concentration in the neutral ground uranium leaching process is solved, achieving It achieves efficient leaching and migration of uranium, shortens the service life of the mining area, and reduces costs.
Patent Information
- Application Number
- CN202211460042.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-11-17
AI Technical Summary
In the neutral uranium leaching process, carbonate minerals react slowly with the neutral leach agent CO2, making it difficult to increase the HCO3- concentration in the ore water, affecting the uranium leaching efficiency. In addition, the HCO3- concentration decreases due to calcite dissolution in the later stages of the mining area. The leaching and migration capabilities of uranium are weakened. Existing solutions such as adding NH4HCO3 or NaHCO3 are costly and make decommissioning management more difficult.
By chemically reacting the uranium mining tail liquid after uranium extraction with carbon dioxide and limestone in a reaction tower, a high bicarbonate leach agent is generated, and an oxygen-rich leach agent is injected into the uranium-containing sandstone layer to promote the leaching of uranium; at the same time, It reacts with carbon dioxide and limestone again in the soaking tank to increase the bicarbonate concentration in the liquid phase in a cycle to meet the requirements of the neutral uranium leaching process.
Economically and effectively increase the bicarbonate concentration in the liquid phase, speed up the leaching rate of uranium, shorten the service life of the mining area, and save material costs by recycling the uranium mining tail liquid and avoid adding new ion components to the Groundwater contamination.
Smart Images

Figure CN115725837B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of mining, in particular to a method and system for neutral leaching of uranium. Background Art
[0002] As of the end of 2021, more than 90% of China's natural uranium production capacity comes from in-situ leaching uranium process. In-situ leaching uranium process has become the mainstream process for my country's current natural uranium production. According to the type of leaching agent used, it can be divided into: acid leaching (H2SO4+H2O2 or H2SO4+O2), alkaline leaching (NaHCO3+Na2CO3) and neutral leaching (CO2+O2 or CO2+O2+NaHCO3 or CO2+O2+NH4HCO3). At present, about 30% to 35% of the natural uranium produced by in-situ leaching uranium in my country comes from the acid leaching process, and 65% to 70% comes from the neutral leaching process. There is no in-situ leaching uranium mine using the alkaline leaching process.
[0003] Neutral in-situ leaching uranium mining technology is generally suitable for ore-bearing layers with high carbonate content (measured in CO2, content> 2%) or groundwater HCO3 in ore-bearing aquifers. - Concentration> 800mg / L in sandstone uranium deposits, and the average pyrite content in the ore-bearing rock layer should be less than 2%. The HCO3 in the ore layer water of most sandstone uranium deposits in my country - The concentration does not meet the requirements of neutral uranium leaching (> 800 mg / L), and is generally only 150-250 mg / L. When neutral leaching of uranium is carried out, a neutral leaching agent "CO2+O2" can be added. CO2 reacts chemically with carbonate minerals to produce Ca(HCO3)2 or Mg(HCO3)2, etc., so that the HCO3 in the ore water - When the concentration increases to above 800 mg / L, uranium can be gradually leached out.
[0004] However, there are two situations: First, when the carbonate minerals in the ore-bearing layer are dolomite, ankerite, etc., they react very slowly with the neutral leaching agent CO2, and the HCO3 in the ore-bearing water - The concentration cannot be significantly increased to 800 mg / L, the uranium leaching is slow, and the migration ability is not strong; secondly, in the middle and late stages of leaching in the mining area, with the dissolution of calcite carbonate minerals, the HCO3 in the ore layer water - The concentration gradually decreased from the original high level to below 800 mg / L, and the uranium leaching and migration capabilities were weakened. To address this problem, NH4HCO3 or NaHCO3 can be directly added to the solution system, but the cost per ton increases by about 2,000 to 3,000 yuan, and the introduction of new ion components increases the difficulty of decommissioning the mining area.
[0005] For HCO3 in the process of neutral leaching of uranium -The problems of low concentration and high cost of directly adding NH4HCO3 or NaHCO3 require the design and invention of an economical and harmless method to increase the bicarbonate concentration of the neutral leaching uranium leaching agent, so as to accelerate the leaching of uranium and shorten the service life of the mining area. Summary of the invention
[0006] The embodiments of the present invention provide a method and system for neutral leaching of uranium, which can improve the efficiency of neutral leaching of uranium economically and effectively.
[0007] According to one aspect of the present invention, there is provided a method for neutral leaching of uranium, comprising:
[0008] A. subjecting the uranium mining tailings after uranium extraction to a first chemical reaction with carbon dioxide and limestone in a reaction tower to generate a recovery leaching agent having a higher bicarbonate concentration than that of the uranium mining tailings:
[0009] CO2+H2O+CaCO3→Ca(HCO3)2
[0010] B. adding oxygen to the recovered leaching agent to obtain an oxygen-enriched leaching agent;
[0011] C. injecting the oxygen-enriched leaching agent into the uranium-containing sandstone ore layer, and generating a second chemical reaction with the uranium ore to generate a uranium-containing leaching solution under a neutral condition of pH 6.5 to 7.5:
[0012] UO2+0.5O2+2HCO3 - →UO2(CO3)2 2- +H2O
[0013] D. the uranium-containing leaching solution undergoes the first chemical reaction with carbon dioxide and limestone in the immersion tank before and / or after uranium extraction to increase the bicarbonate concentration;
[0014] The concentration of carbon dioxide in step A is 200-600 mg / L;
[0015] The concentration of oxygen in step B is 50-300 mg / L.
[0016] Preferably, in any embodiment,
[0017] When the injection pressure of the uranium mining tailings in step A increases to 1.6 MPa, the reaction tower is flushed.
[0018] Preferably, in any embodiment,
[0019] When the pressure of carbon dioxide in the reaction tower exceeds 1.6 MPa, exhaust is performed.
[0020] Preferably, in any embodiment,
[0021] Execute step A multiple times before executing step B.
[0022] According to another aspect of the present invention, there is provided a neutral leaching uranium system for operating the neutral leaching uranium method as described above, comprising:
[0023] A reaction tower, comprising an upper liquid inlet, a lower liquid discharge port, a limestone reaction layer arranged between the liquid inlet and the liquid discharge port, and a carbon dioxide inlet port introduced into the limestone reaction layer, wherein the uranium leaching agent entering from the liquid inlet undergoes a first chemical reaction with carbon dioxide and limestone in the limestone reaction layer to generate a recovered leaching agent with a higher bicarbonate concentration, which is discharged from the liquid discharge port;
[0024] The immersion tank is filled with limestone for the uranium-containing leaching solution flowing out of the uranium-containing sandstone ore layer to undergo a first chemical reaction with carbon dioxide and limestone to generate a uranium-containing leaching agent with a higher bicarbonate concentration.
[0025] Preferably, in any embodiment,
[0026] The reaction tower comprises a plurality of reaction towers connected in series.
[0027] Preferably, in any embodiment,
[0028] The reaction towers include multiple groups of reaction towers for parallel processing, and each group of reaction towers includes multiple reaction towers connected in series.
[0029] Preferably, in any embodiment,
[0030] The limestone reaction layer of the reaction tower includes quartz sand, wherein the ratio of limestone to quartz sand is 3:1 to 2:1.
[0031] The neutral uranium leaching method and system provided by the embodiments of the present invention can increase the bicarbonate concentration in the liquid phase system, and can economically and effectively improve the efficiency of neutral uranium leaching. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be discussed below. Obviously, the technical solutions described in conjunction with the drawings are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments and their drawings can be obtained based on the embodiments shown in these drawings without paying creative work.
[0033] Figure 1 is a flow chart of a method for neutral leaching of uranium according to an embodiment of the present invention. DETAILED DESCRIPTION
[0034] The technical solutions of various embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments described in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The embodiments of the present invention provide a method and system for neutral leaching of uranium, which can improve the efficiency of neutral leaching of uranium economically and effectively.
[0036] According to one aspect of the present invention, there is provided a method for neutral leaching of uranium, comprising:
[0037] A. subjecting the uranium mining tailings after uranium extraction to a first chemical reaction with carbon dioxide and limestone in a reaction tower to generate a recovery leaching agent having a higher bicarbonate concentration than that of the uranium mining tailings:
[0038] CO2+H2O+CaCO3→Ca(HCO3)2
[0039] B. adding oxygen to the recovered leaching agent to obtain an oxygen-enriched leaching agent;
[0040] C. injecting the oxygen-enriched leaching agent into the uranium-containing sandstone ore layer, and generating a second chemical reaction with the uranium ore to generate a uranium-containing leaching solution under a neutral condition of pH 6.5 to 7.5:
[0041] UO2+0.5O2+2HCO3 - →UO2(CO3)2 2- +H2O
[0042] D. The uranium-containing leaching solution undergoes the first chemical reaction with carbon dioxide and limestone in the leaching pool before and / or after uranium extraction to increase the bicarbonate concentration.
[0043] In this way, the uranium mining tailings undergo a first chemical reaction with carbon dioxide and limestone in a reaction tower to increase the bicarbonate concentration in the liquid phase, meeting the requirements of the neutral uranium leaching process (the bicarbonate concentration is greater than 800 mg / L), and the uranium-containing leaching solution (before and / or after uranium extraction) generated after the leaching agent is injected into the uranium-containing sandstone ore layer to undergo a second chemical reaction is again subjected to a first chemical reaction with carbon dioxide and limestone in a soaking tank to increase the bicarbonate concentration in the liquid phase, and finally a uranium mining tailing with a high bicarbonate concentration is obtained. Thus, the cyclic operation can not only economically and effectively increase the bicarbonate concentration in the liquid phase through the chemical reaction with carbon dioxide and limestone to meet the requirements of the neutral uranium leaching process, but also the uranium mining tailings can be recycled, which can save material costs.
[0044] In addition, adding carbon dioxide to the reaction tower and maintaining a relatively high pressure can accelerate the dissolution reaction (ie, the first chemical reaction). At the same time, the solution flows faster under pressure and does not cause the deposition of excess calcium ions.
[0045] In addition, the use of residual CO2·H2O in the leaching solution in the immersion tank can further improve the utilization efficiency of carbon dioxide. At the same time, the longer residence time of the leaching solution in the immersion tank can significantly increase the bicarbonate concentration in the solution system without pressurization.
[0046] It can be seen that the neutral uranium leaching method and system provided by the embodiments of the present invention can increase the bicarbonate concentration in the liquid phase system to accelerate the leaching of uranium and shorten the service life of the mining area, thereby being able to economically and effectively improve the efficiency of neutral uranium leaching.
[0047] Optionally, in any embodiment, the first chemical reaction in the soaking tank described in step D is: the uranium-containing leachate is subjected to a first chemical reaction with carbon dioxide and limestone in the soaking tank before uranium extraction to increase the bicarbonate concentration. Then, the uranium-containing leachate with a high bicarbonate concentration can be used for uranium extraction (for example, uranium adsorption is performed by an adsorption tower), and the depleted uranium tail liquid after uranium extraction can be returned to step A for treatment to achieve recycling.
[0048] Optionally, in any embodiment, the first chemical reaction in the soaking tank in step D is: after uranium extraction (for example, uranium adsorption by an adsorption tower), the uranium-containing leaching solution produces depleted uranium tail liquid, and the depleted uranium tail liquid undergoes a first chemical reaction with carbon dioxide and limestone in the soaking tank to increase the bicarbonate concentration. Then, the depleted uranium tail liquid with a high bicarbonate concentration can be returned to step A for treatment to achieve recycling.
[0049] Preferably, in any embodiment, the concentration of carbon dioxide in step A is 200-600 mg / L (the concentration can be set based on the volume of the solution).
[0050] Preferably, in any embodiment, the concentration of oxygen in step B is 50-300 mg / L (the concentration can be set based on the volume of the solution).
[0051] The reaction tower can filter out fine muddy particles in the uranium mining tail liquid, absorb impurities such as organic matter, silicon-containing and iron-containing colloids, and play a role in intercepting impurities and purifying the solution. In actual use, the limestone particles and quartz sand particles in the limestone reaction layer in the reaction tower can absorb organic matter and silicon-containing and iron-containing colloids in the solution. In addition, the liquid flows from the external pipeline into the limestone reaction layer with a porous structure in the reaction tower, and the flow rate is slowed down, which can also play a certain sedimentation role to facilitate the removal of impurities in the solution.
[0052] In view of this, it is necessary to regularly flush the reaction tower to eliminate the impurities removed from the solution to ensure the effectiveness of purifying the solution.
[0053] Preferably, in any embodiment, when the injection pressure of the uranium mining tailings in step A increases to 1.6 MPa, the reaction tower is flushed.
[0054] Optionally, in any embodiment, the reaction tower is flushed with high-pressure clean water.
[0055] Optionally, in any embodiment, the flushing pressure of the reaction tower is 2.0-5.0 MPa.
[0056] Preferably, in any embodiment, when the pressure of carbon dioxide in the reaction tower exceeds 1.6 MPa, exhaust is performed.
[0057] Optionally, in any embodiment, if the reaction tower needs flushing due to blockage, the flushing is performed after venting.
[0058] Preferably, in any embodiment, step A is performed multiple times before step B is performed.
[0059] Optionally, in any embodiment, the total execution time of step A may be at least 30 minutes.
[0060] According to another aspect of the present invention, there is provided a neutral leaching uranium system for operating the neutral leaching uranium method as described above, comprising:
[0061] A reaction tower, comprising an upper liquid inlet, a lower liquid discharge port, a limestone reaction layer arranged between the liquid inlet and the liquid discharge port, and a carbon dioxide inlet port introduced into the limestone reaction layer, wherein the uranium leaching agent entering from the liquid inlet undergoes a first chemical reaction with carbon dioxide and limestone in the limestone reaction layer to generate a recovered leaching agent with a higher bicarbonate concentration, which is discharged from the liquid discharge port;
[0062] The immersion tank is filled with limestone for the uranium-containing leaching solution flowing out of the uranium-containing sandstone ore layer to undergo a first chemical reaction with carbon dioxide and limestone to generate a uranium-containing leaching agent with a higher bicarbonate concentration.
[0063] In this way, the uranium mining tailings (or uranium mining leaching agents or recovered leaching agents) undergo a first chemical reaction with carbon dioxide and limestone in a reaction tower to increase the bicarbonate concentration in the liquid phase to meet the neutral uranium leaching process requirements (bicarbonate concentration is greater than 800 mg / L); the uranium-containing leaching solution (before and / or after uranium extraction) generated after the leaching agent is injected into the uranium-containing sandstone ore layer to undergo a second chemical reaction can be subjected to a first chemical reaction again with carbon dioxide and limestone in a soaking tank to increase the bicarbonate concentration in the liquid phase, and finally obtain a uranium mining tailing with a high bicarbonate concentration. In this cyclic operation, not only can the bicarbonate concentration in the liquid phase be economically and effectively increased by chemical reaction with carbon dioxide and limestone to meet the neutral uranium leaching process requirements, but the uranium mining tailings can also be recycled, saving material costs.
[0064] It can be seen that the neutral uranium leaching method and system provided by the embodiments of the present invention can increase the bicarbonate concentration in the liquid phase system to accelerate the leaching of uranium and shorten the service life of the mining area, thereby being able to economically and effectively improve the efficiency of neutral uranium leaching.
[0065] Preferably, in any embodiment, the reaction tower comprises a plurality of reaction towers connected in series (e.g., three reaction towers are arranged in series). In this way, the uranium mining tailings (or uranium mining leaching agent or recovered leaching agent) are sequentially subjected to the first chemical reaction in a plurality of reaction towers to gradually increase the bicarbonate concentration, which is particularly suitable for applications with a large flow rate. It should be understood that the size and quantity of the reaction towers can be set accordingly according to the required flow rate.
[0066] Preferably, in any embodiment, the reaction tower comprises a plurality of groups of reaction towers for parallel processing, and each group of reaction towers comprises a plurality of reaction towers connected in series. In this way, the solution processing capacity can be further enhanced.
[0067] In order to prevent possible scaling problems in the reaction tower and soaking tank, a certain proportion of skeleton support material particles (such as quartz sand, fine expanded clay, or other inactive particles, etc.) can be added to the limestone to form a skeleton structure to support the limestone and prevent it from becoming muddy due to chemical reactions, thereby maintaining good porosity and permeability in the limestone layer, which is conducive to the continuous first chemical reaction.
[0068] Preferably, in any embodiment, the limestone reaction layer of the reaction tower includes quartz sand, wherein the weight ratio of limestone to quartz sand is 3:1 to 2:1.
[0069] Optionally, in any embodiment, the particle size of the limestone and quartz sand in the limestone reaction layer of the reaction tower is 2-5 mm.
[0070] Optionally, in any embodiment, quartz sand is provided in the soaking pool.
[0071] Optionally, in any embodiment, the weight ratio of limestone to quartz sand in the soaking pool is 5:1 to 3:1.
[0072] Optionally, in any embodiment, the particle size of the limestone and quartz sand in the soaking pool is 2-5 mm.
[0073] Optionally, in any embodiment, a coarse gravel cushion layer is provided at the bottom of the reaction tower, and the coarse gravel cushion layer is separated from the limestone reaction layer above it by a predetermined distance.
[0074] Optionally, in any embodiment, the coarse gravel cushion layer of the reaction tower is separated from the limestone reaction layer above it by a grid-like partition.
[0075] Optionally, in any embodiment, a waste liquid discharge pipe is provided at the bottom of the reaction tower to discharge the waste water after flushing the reaction tower into a waste liquid recovery pool.
[0076] Figure 1 is a flow chart of a method for neutral leaching of uranium according to an embodiment of the present invention.
[0077] exist Figure 1 In the embodiment shown, a method for neutral leaching of uranium can be seen, comprising:
[0078] Step 110: The uranium mining tail liquid after uranium extraction is subjected to a first chemical reaction with carbon dioxide and limestone in the reaction tower to generate a recovery leaching agent having a higher bicarbonate concentration than that of the uranium mining tail liquid:
[0079] CO2+H2O+CaCO3→Ca(HCO3)2
[0080] Step 120. adding oxygen to the recovered leaching agent to obtain an oxygen-enriched leaching agent;
[0081] Step 130: inject the oxygen-enriched leaching agent into the uranium-containing sandstone ore layer, and generate a second chemical reaction with the uranium ore under a neutral condition of pH 6.5 to 7.5 to generate a uranium-containing leaching solution:
[0082] UO2+0.5O2+2HCO3 - →UO2(CO3)2 2- +H2O
[0083] Step 140. The uranium-containing leaching solution undergoes the first chemical reaction with carbon dioxide and limestone in the leaching tank before and / or after uranium extraction to increase the bicarbonate concentration.
[0084] In a preferred embodiment, a method for neutral leaching of uranium comprises:
[0085] (1) Carbon dioxide gas (such as liquid storage) is introduced into a carbonate reaction tower (i.e., the reaction tower) filled with "quartz stone + quartz sand" in an amount of 200 to 600 mg / L.
[0086] (2) The uranium mining tailings (which can come from the tailings recovery pool) undergo the first chemical reaction with carbon dioxide and limestone in the reaction tower:
[0087] CO2+H2O+CaCO3→Ca(HCO3)2 (Formula 1)
[0088] The bicarbonate concentration in the uranium mining tailings is increased through chemical reactions (in practice, the first chemical reaction can be repeated multiple times to gradually increase the bicarbonate concentration), forming a recovered leaching agent that is transported to the injection control room in the mining area.
[0089] In the case of three reaction towers in series, the total contact time between the solution of the three towers in series and the limestone should be guaranteed to be ≥30min; the size and number of the reaction towers should be designed according to the required flow rate. When the processing flow rate is large, multiple rows (multiple groups) of three towers in series can be used.
[0090] The reaction tower is filled with a mixture of "limestone + quartz sand" with a particle size of 2 to 5 mm and a ratio of limestone to quartz sand of 3:1 to 2:1; the bottom of the reaction tower is filled with a coarse gravel cushion layer, and between the cushion layer and the upper fine-grained "limestone and quartz sand" is a grid-like partition.
[0091] In addition to the first chemical reaction of formula 1, the reaction tower can also filter out fine muddy particles in the tail liquid, adsorb organic matter, silicon-containing and iron-containing colloids and other impurities, thereby purifying the solution; because the reaction tower has the function of intercepting impurities in the tail liquid, the reaction tower needs to be flushed regularly.
[0092] (3) Oxygen (e.g., storable in liquid form) is introduced into the injection branch pipe of each injection well at a concentration of 50 to 300 mg / L.
[0093] (4) Injecting an oxygen-rich leaching agent rich in bicarbonate and oxygen into the uranium-bearing sandstone reservoir, a second chemical reaction occurs under neutral conditions of pH 6.5 to 7.5:
[0094] UO2+0.5O2+2HCO3 - → UO2(CO3)2 2- +H2O (Formula 2)
[0095] Uranium minerals are oxidized and leached by complexation, and accumulate continuously on the path from the injection well to the extraction well, obtaining a high concentration of UO2(CO3)2 2-Leachate: The uranium-containing leachate is pumped out to the surface through the extraction well, gathered in the extraction control room of the mining area, and transported to the leachate collection pool by gravity or injection pumps.
[0096] (5) The leachate undergoes a first chemical reaction with the limestone in the immersion tank (as shown in Formula 1). A large amount of CO2·H2O exists in the leachate, and the concentration of bicarbonate in the leachate is increased.
[0097] Usually, the leachate collection pool of neutral leaching uranium is only used to collect and store the leachate extracted from each mining area. In the embodiment of the present invention, limestone with a particle size of 2 to 5 mm and quartz sand are mixed in a ratio of 5:1 to 3:1, and paved to the bottom of the leachate collection pool with a paving thickness of 20 cm to 50 cm, forming a leachate collection pool different from the general neutral leaching uranium mine, so it is called a carbonate leaching pool. In the leaching pool, the leachate and limestone maintain a certain ratio of inflow and outflow, but the pool always maintains 3 to 5 times the volume of limestone. Therefore, in the limestone leaching pool, the bicarbonate concentration of the leachate can be greatly improved (for example, it can be increased from 400 to 600 mg / L to 900 to 1100 mg / L).
[0098] The leaching liquid is transported from the immersion tank to the adsorption towers of the water smelting plant through the injection pump to adsorb uranium, and the depleted uranium tail liquid is injected into the tail liquid recovery pool.
[0099] It should be understood that the limestone soaking process (soaking pool) described in the present invention can also be set in the tailings pool, which can also increase the bicarbonate concentration of the tailings, and can be determined according to the convenience of the mine.
[0100] The effects of the present invention are further illustrated and verified by three groups of indoor tests.
[0101] 200 mg / L carbon dioxide was passed into three beakers containing 200 mL of distilled water, 50 g of calcite + 200 mL of distilled water, and 50 g of limestone + 200 mL of distilled water, respectively. Samples were taken twice every 6 h and 12 h to determine the HCO3 in the solution. - Concentration, Ca 2 + The concentration and analysis methods are JS / FX / 8.2-04 / N / 2004 and JY / T015-1996 respectively.
[0102] Among them, the particle size of calcite is 1 to 2 mm, and the particle size of limestone is 2 to 5 mm.
[0103] The experimental results and analysis are shown in the table:
[0104]
[0105] Indoor tests have shown that low-concentration carbon dioxide can dissolve calcite and limestone in a shorter period of time, with limestone dissolving faster. Therefore, limestone can be given priority in field applications.
[0106] At the same time, in order to prevent scaling problems that may be caused by the reaction tower and the soaking tank, a certain proportion of quartz sand can be added to the limestone to maintain good porosity and permeability. Adding carbon dioxide to the reaction tower and maintaining a high pressure can accelerate the dissolution reaction, and the solution flows faster, which will not cause excess calcium ion deposition. The use efficiency of CO2 can be further improved by using the residual CO2·H2O in the leaching solution in the soaking tank. At the same time, the residence time of the leaching solution in the soaking tank is used to increase the bicarbonate in the solution system.
[0107] In a neutral leaching area, if the bicarbonate in the leaching solution is 550 mg / L, it can be increased to 800-1000 mg / L through the scheme of the present invention, meeting the optimal complexing conditions for uranium ore leaching, thereby accelerating the leaching of uranium.
[0108] In view of the decrease in carbonate content in the uranium-bearing sandstone reservoir in the middle and late stages of leaching in the mining area or the insufficient carbonate content in the original sandstone reservoir, it is necessary to supplement carbonate to increase the bicarbonate concentration in the solution system. Among the compound materials that can increase the bicarbonate concentration, the main component of limestone is calcium carbonate, which costs about 40 to 150 yuan per ton, only 1 / 20 of NH4HCO3 or NaHCO3, so it can be used as a substitute for traditional materials and is an economical and effective choice.
[0109] The present invention increases the bicarbonate concentration in the neutral uranium leaching solution through chemical reactions in a carbonate soaking tank and a carbonate reaction tower, achieves an increase in the bicarbonate concentration in the neutral uranium leaching solution system without increasing or changing the ion components in the neutral leaching solution system, can accelerate the dissolution and migration of uranium ore, increase the leaching rate of uranium, and shorten the service life of the mining area.
[0110] In addition, the present invention adopts a carbonate supplement method (i.e., limestone) that is as close to natural conditions as possible to increase the bicarbonate concentration in the solution system. It does not add "NH4HCO3" as in the prior art, thereby causing less pollution to groundwater and reducing the cost of treatment for later decommissioning of the mining area; nor does it adopt the method of adding "NaHCO3" as in the prior art, thereby not causing clay mineral expansion.
[0111] The neutral uranium leaching method and system provided by the embodiments of the present invention can increase the bicarbonate concentration in the system, and can economically and effectively improve the efficiency of neutral uranium leaching.
[0112] It should be noted that, in this article, relational terms such as first and second are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements not only includes these elements, but also includes other elements not clearly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements limited by the sentence "comprise a ..." do not exclude the existence of other identical factors in the process, method, article or equipment including the elements.
[0113] In the description of multiple elements herein, multiple parallel features connected by "and / or" refer to one or more (or one or more) of these parallel features. For example, "the first element and / or the second element" means: one or more of the first element and the second element, that is, only the first element, or only the second element, or the first element and the second element (both exist at the same time).
[0114] The various embodiments provided in the present invention can be combined with each other as needed. For example, the features of any two, three or more embodiments can be combined with each other to form a new embodiment of the present invention. This is also within the scope of protection of the present invention, unless otherwise stated or technically inconsistent and cannot be implemented.
[0115] The above description is only an exemplary embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for neutral leaching of uranium, characterized in that: include: A. subjecting the uranium mining tailings after uranium extraction to a first chemical reaction with carbon dioxide and limestone in a reaction tower to generate a recovery leaching agent having a higher bicarbonate concentration than that of the uranium mining tailings: CO2+H2O+CaCO3→Ca(HCO3)2 B. adding oxygen to the recovered leaching agent to obtain an oxygen-enriched leaching agent; C. injecting the oxygen-enriched leaching agent into the uranium-containing sandstone ore layer, and generating a second chemical reaction with the uranium ore to generate a uranium-containing leaching solution under a neutral condition of pH 6.5 to 7.5: <h2 style=";text-align:left;direction:ltr">UO2+0.5O2+2HCO3<h2 style=";text-align:left;direction:ltr"> - <h2 style=";text-align:left;direction:ltr"> →UO2(CO3)2<h2 style=";text-align:left;direction:ltr"> 2- <h2 style=";text-align:left;direction:ltr"> +H2O D. the uranium-containing leaching solution undergoes the first chemical reaction with carbon dioxide and limestone in the immersion tank before and / or after uranium extraction to increase the bicarbonate concentration; The concentration of carbon dioxide in step A is 200-600 mg / L; The concentration of oxygen in step B is 50-300 mg / L.
2. The neutral leaching method for uranium according to claim 1, characterized in that: Further including: When the injection pressure of the uranium mining tailings in step A increases to 1.6 MPa, the reaction tower is flushed.
3. The neutral leaching method for uranium according to claim 1, characterized in that: Further including: When the pressure of carbon dioxide in the reaction tower exceeds 1.6 MPa, exhaust is performed.
4. The neutral leaching method for uranium according to claim 1, characterized in that: Execute step A multiple times before executing step B.
5. A neutral uranium leaching system for operating the neutral uranium leaching method according to any one of claims 1 to 4, characterized in that: include: A reaction tower, comprising an upper liquid inlet, a lower liquid discharge port, a limestone reaction layer arranged between the liquid inlet and the liquid discharge port, and a carbon dioxide inlet port introduced into the limestone reaction layer, wherein the uranium leaching agent entering from the liquid inlet undergoes a first chemical reaction with carbon dioxide and limestone in the limestone reaction layer to generate a recovered leaching agent with a higher bicarbonate concentration, which is discharged from the liquid discharge port; The immersion tank is filled with limestone for the uranium-containing leaching solution flowing out of the uranium-containing sandstone ore layer to undergo a first chemical reaction with carbon dioxide and limestone to generate a uranium-containing leaching agent with a higher bicarbonate concentration.
6. The neutral in-situ leaching system for uranium mining according to claim 5, characterized in that: The reaction tower comprises a plurality of reaction towers connected in series.
7. The neutral in-situ leaching system for uranium mining according to claim 5, characterized in that: The reaction towers include multiple groups of reaction towers for parallel processing, and each group of reaction towers includes multiple reaction towers connected in series.
8. The neutral in-situ leaching system for uranium mining according to claim 5, characterized in that: The limestone reaction layer of the reaction tower includes quartz sand, wherein the ratio of limestone to quartz sand is 3:1 to 2:1.
Citation Information
Patent Citations
Uranium extraction from underground deposits
CA1117862A