MIM powder and MIM molding process of 1800MPa ultra-high strength and high toughness steel

A MIM powder and process with specific metal compositions and treatments achieve ultra-high strength and toughness steel parts, addressing the limitations of existing MIM technologies for high-performance applications.

CN115740427BActive Publication Date: 2024-12-03SHENZHEN ELEMENT TECH CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211523867.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-30
Publication Date
2024-12-03
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

Existing MIM processes struggle to produce metal parts with both ultra-high strength (≥1800MPa) and high toughness (≥5% elongation) suitable for high-performance applications in industries such as 3C, tools, and automobiles, particularly for foldable screen mobile phone hinges.

Method used

A MIM powder composition of C 0.0-0.6%, Cr 2.0-3.5%, Ni 11.0-14.0%, Co 14.0-17.0%, Mo 1.5-2.5% with a particle size ≤50μm, combined with a forming process involving kneading, injection molding, catalytic debinding, thermal debinding, sintering, and treatments like solution treatment, cryogenic treatment, and aging to achieve the desired properties.

Benefits of technology

The process results in ultra-high strength and toughness steel parts with yield strength ≥1800MPa, elongation ≥5%, and hardness of 52-58HRC, suitable for high-performance applications with high production efficiency and dimensional consistency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of metal powder injection molding, and particularly relates to a MIM powder and MIM molding process of 1800MPa ultra-high strength and high toughness steel. The MIM powder is composed of the following metal powders in weight percentage: 0.0-0.6% C, 2.0-3.5% Cr, 11.0-14.0% Ni, 14.0-17.0% Co, 1.5-2.5% Mo, and the remainder Fe and impurities, and the particle size of the MIM powder is ≤50μm. The MIM molding process prepares ultra-high strength and high toughness steel parts with a yield strength of ≥1800MPa, an elongation of ≥5%, and a hardness of 52-58HRC by improving the raw material composition and the thermal degreasing and sintering processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal powder injection molding, and in particular relates to a MIM powder and a MIM molding process of 1800MPa-grade ultra-high strength and high-toughness steel. Background Art

[0002] As consumers' demands for the functions of mobile smart terminals continue to upgrade, foldable screen mobile phones have become a new growth point for smart phones. The foldable screen solution can well balance the contradiction between large screen and small size, giving smart phones a more fashionable appearance and a richer user experience. However, the weight of foldable screen mobile phones is heavier than that of traditional mobile phones, which will reduce the portability of mobile phones to a certain extent and affect the user experience. Without affecting the functions of foldable screen mobile phones, the use of more precise, thinner and high-strength hinges is one of the important ways to reduce the weight of foldable screen mobile phones. At present, the 17-4PH and 420W stainless steels commonly used in the hinges of foldable screen mobile phones are difficult to meet the needs of hinge thinning and strengthening due to the ultimate strength of the material itself. Therefore, it is urgent to develop an ultra-high strength and high-toughness steel with high strength, high toughness and good fatigue resistance for the production of high-precision hinges to achieve the effect of weight reduction of foldable screen mobile phones.

[0003] Metal Powder Injection Molding (MIM) technology is a new powder metallurgy molding technology formed by introducing modern plastic injection technology into the field of powder metallurgy. MIM technology uses mold injection molding blanks and quickly manufactures high-precision, three-dimensional complex parts through sintering. It is particularly suitable for mass production and is widely used in the production of hinge parts for folding screen mobile phones.

[0004] At present, it is difficult for metal parts formed by MIM technology to meet the requirements of ultra-high strength and high toughness at the same time. The Chinese invention patent with application number 202010154524.1 discloses an injection molding method for high-strength and high-toughness metal parts. The material composition is Ni 17.0-18.0%, Co 8.5-9.5%, Mo 4.5-5%, and the balance is Fe. After sintering and heat treatment, the yield strength only reaches 1350MPa and the elongation is 6%; the Chinese invention patent with application number 202010852638.3 discloses an injection molded ultra-high strength steel with a material composition of C <0.1%, Ni 15.5-19.5%, Co 7.0-10.0%, Mo 4.0~6.0%, Ti<1.5%, and the balance is Fe. Although the yield strength can reach 1500MPa level, the maximum elongation is only 6%, and with the increase of yield strength, the elongation decreases; Chinese invention patent with application number 202010200648.9 discloses a MIM process for complex corrosion-resistant steel parts, the material composition is C<0.1%, Cr 11.0~15.0%, Ni10.0~14.0%, Mo 0.5~2.0%, Si<0.5%, Mn<0.5%, Ti 1.0~4.0%, and the balance is Fe. The elongation of the material after heat treatment is 12~13%, but the yield strength only reaches 1500MPa; Chinese invention patent with application number 201410248360.3 discloses a method for metal powder injection molding high-strength maraging steel, the material composition is C≤0.08%, Ni 17.0~19.0%, Co 8.0~10.0%, Mo 4.5~6.5%, the balance is Fe and inevitable impurities. Although the elongation is ≥10%, the strength is still low, and only the tensile strength can reach 1500MPa.

[0005] Therefore, it is of great technical and economic significance to develop a MIM forming process for ultra-high strength and high toughness steel parts with a yield strength ≥1800MPa and an elongation ≥5% to manufacture metal parts with ultra-high strength, high toughness and complex three-dimensional shapes to meet the needs of 3C, tools, automobiles and other industries for high-performance parts. Summary of the invention

[0006] In order to overcome the defects of the prior art mentioned above, the technical problem to be solved by the present invention is to provide a MIM powder and MIM molding process of 1800MPa grade ultra-high strength and high toughness steel.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a MIM powder of 1800MPa grade ultra-high strength and high toughness steel, comprising the following metal powders in weight percentage: C 0.0-0.6%, Cr2.0-3.5%, Ni 11.0-14.0%, Co 14.0-17.0% and Mo 1.5-2.5%, and the particle size of the MIM powder is ≤50μm.

[0008] Another technical solution of the present invention is: a MIM forming process of 1800MPa grade ultra-high strength and high toughness steel, comprising the following steps:

[0009] S1: kneading the MIM powder and the binder to obtain a feed material, and then crushing and / or granulating the feed material;

[0010] S2: injection molding the crushed and / or granulated feed into a green body;

[0011] S3: catalytically debinding the green body;

[0012] S4: The green body after catalytic debinding is subjected to thermal debinding, deoxidation and decarburization and sintering in an inert gas atmosphere of 0 to 50 kPa in sequence to obtain a sintered part;

[0013] S5: The sintered parts are subjected to solution treatment, cryogenic treatment and aging treatment in sequence to obtain ultra-high strength and high toughness steel.

[0014] The beneficial effects of the present invention are as follows: the MIM forming process of the 1800MPa-level ultra-high strength and high-toughness steel parts provided by the present invention, by improving the raw material composition and the hot degreasing and sintering process, prepares ultra-high strength and high-toughness steel parts with a yield strength ≥1800MPa, an elongation ≥5%, and a hardness of 52-58HRC. The process is simple, economical, and efficient, and can mass-produce metal parts with ultra-high strength, high toughness, and high hardness and three-dimensional complex shapes in a short period of time. The strength and hardness of the obtained ultra-high strength and high-toughness steel parts are significantly higher than those of the steel parts prepared by the existing MIM process, so that it can meet the needs of 3C, tools, automobiles and other industries for high-performance parts, and is particularly suitable for mass production of metal parts with complex three-dimensional shapes and high performance requirements. DETAILED DESCRIPTION

[0015] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in conjunction with the implementation modes.

[0016] The key concept of the present invention is that by improving the raw material composition and the hot degreasing and sintering processes, ultra-high strength and high toughness steel parts with a yield strength of ≥1800MPa, an elongation of ≥5%, and a hardness of 52-58HRC are prepared.

[0017] The invention discloses an MIM powder of 1800MPa ultra-high strength and high toughness steel, comprising the following metal powders in weight percentage: C 0.0-0.6%, Cr 2.0-3.5%, Ni 11.0-14.0%, Co 14.0-17.0% and Mo 1.5-2.5%, and the particle size of the MIM powder is ≤50μm.

[0018] From the above description, it can be seen that the beneficial effects of the present invention are: Co in MIM powder is an element that improves the strength of steel. Through the synergistic effect with Mo element, the strength of steel can be improved, but the contribution to toughness is very small; Ni is an element that improves the toughness of steel, but Ni element will lower the Ms point of steel, which is not conducive to the formation of full martensite; therefore, the use of a specific ratio of Co and Ni metals is a prerequisite for ensuring that the steel has high strength and high toughness.

[0019] Furthermore, the metal powder comprises the following weight percentages: C 0.1-0.4%, Cr 2.0-3.5%, Ni 11.0-13.0%, Co 15.0-17.0% and Mo 1.5-2.0%, and the particle size of the MIM powder is ≤25 μm.

[0020] From the above description, it can be seen that by more accurately controlling each element in the raw material components, the strength, toughness and hardness of the resulting steel parts can be further improved.

[0021] Furthermore, it also includes impurities with a weight percentage of 0-2.02% and the balance of iron.

[0022] Furthermore, the weight percentage of each element in the impurities to the weight of the MIM powder is as follows: Mn≤1.0%, Si≤1.0%, S≤0.01% and P≤0.01%.

[0023] Another technical solution of the present invention is: a MIM forming process of 1800MPa grade ultra-high strength and high toughness steel, comprising the following steps:

[0024] S1: kneading the MIM powder and the binder to obtain a feed material, and then crushing and / or granulating the feed material;

[0025] S2: injection molding the crushed and / or granulated feed into a green body;

[0026] S3: catalytically debinding the green body;

[0027] S4: The green body after catalytic debinding is subjected to thermal debinding, deoxidation and decarburization and sintering in an inert gas atmosphere of 0 to 50 kPa in sequence to obtain a sintered part;

[0028] S5: The sintered parts are subjected to solution treatment, cryogenic treatment and aging treatment in sequence to obtain ultra-high strength and high toughness steel.

[0029] From the above description, it can be seen that the beneficial effects of the present invention are: the MIM forming process of the ultra-high strength and high toughness steel parts provided by the present invention adopts a specific proportion of raw material components to prepare a green body, and then sequentially undergoes catalytic degreasing, thermal degreasing, deoxidation and decarburization, sintering, solid solution treatment, deep cryogenic treatment and aging treatment, so that the components in the alloy can be evenly dissolved into the matrix to form a uniform solid solution, which has the effect of improving the elongation, so as to obtain an ultra-high strength and high toughness steel with a yield strength of ≥1800MPa, an elongation of ≥5%, and a hardness of 52 to 58HRC, which can meet the requirements of 3C, tools, automobiles, aerospace and other industries for ultra-high strength, high toughness and wear-resistant parts, and has the advantages of high production efficiency, low cost, and good dimensional consistency.

[0030] Catalytic degreasing before sintering can remove most of the binder in the green body, preventing the green body from cracking, bulging, deformation or collapse during the sintering process. Being in an inert atmosphere can prevent the metal powder from reacting with oxygen in the air and oxidizing.

[0031] Furthermore, the specific steps of thermal degreasing are: raising the ambient temperature from room temperature to 250-350°C at a heating rate of 0.1-10°C / min, and keeping it warm for 0-180min; continuing to raise the temperature to 400-500°C at a heating rate of 0.1-10°C / min, and keeping it warm for 0-180min; continuing to raise the temperature to 550-800°C at a heating rate of 0.1-10°C / min, and keeping it warm for 0-180min.

[0032] From the above description, it can be seen that the high temperature treatment of 500-800°C in thermal degreasing can decompose the remaining binder after catalytic degreasing by heat, thereby preventing the binder residue from being cracked into carbon and oxygen in the subsequent high temperature treatment and affecting the final performance of the material.

[0033] Thermal degreasing in an inert atmosphere can prevent metal powder from reacting with oxygen in the air and causing oxidation.

[0034] If the heating rate during the thermal degreasing process is too low, the thermal degreasing time will be prolonged and the thermal degreasing efficiency will be reduced; if the heating rate is too fast, the binder will decompose and volatilize violently, resulting in defects such as cracks and bulging, and the binder will not be removed and will be carbonized.

[0035] If the thermal degreasing temperature is too low, the binder in the degreased embryo will not be completely removed, resulting in a high carbon content in the material; if the thermal degreasing temperature is too high, the low molecular weight components in the binder will decompose and volatilize violently, which may easily cause defects such as cracks and bulges.

[0036] Furthermore, the specific steps of deoxidation and decarburization are: controlling the gas pressure in the furnace to be less than 10Pa, raising the ambient temperature from 500-800°C to 900-1200°C at a heating rate of 0.1-8°C / min, and then keeping the temperature for 10-240 minutes.

[0037] From the above description, it can be seen that some oxygen will inevitably exist in the metal powder. Oxygen is an impurity element in steel, which is not conducive to sintering densification and reduces the strength and toughness of steel. The removal of oxygen mainly relies on the reaction of carbon and oxygen to generate CO during the sintering process, which is removed in the form of gas. Carbon in the material is an important strengthening element. Too high a carbon content will cause a large amount of carbides to precipitate at the grain boundaries of the steel, which will have an adverse effect on the toughness of the steel. Too low a carbon content will reduce the strength of the material. Therefore, it is necessary to control the carbon content in the steel within a more appropriate range and carry out deoxidation and decarburization treatment.

[0038] Furthermore, the specific steps of sintering are: raising the ambient temperature from 900-1200°C to 1320-1380°C at a heating rate of 0.1-10°C / min, then keeping the temperature for 30-360 minutes, and then cooling to room temperature to obtain a sintered part.

[0039] From the above description, it can be seen that if the sintering temperature is too low, the material cannot be densified; if the sintering temperature is too high, the material will be over-burned or melted. If the heating rate during the sintering process is too slow, the sintering efficiency will be reduced; if the heating rate is too fast, the pores in the degreased embryo cannot be discharged in time, the sintering is not dense, the porosity increases, and the material performance is affected.

[0040] Furthermore, the specific steps of the solution treatment are: placing the sintered part in a vacuum environment, keeping the temperature at 950-1150°C for 10-180 minutes, and then cooling it to room temperature, the cooling medium is nitrogen and / or argon, the cooling rate is ≥50°C / min, and the pressure of the cooling medium is 100-1000 kPa.

[0041] From the above description, it can be seen that solution treatment, cryogenic treatment and aging treatment are the key steps to form martensite, martensitic phase transformation and carbide precipitation; the appropriate temperature and holding time in solution treatment combined with rapid cooling can ensure that the components in the alloy can be evenly dissolved into the matrix to form a uniform solid solution, which has the effect of improving elongation. Solution treatment has requirements for gas pressure in the cooling stage. The higher the gas pressure, the faster the cooling rate and the more uniform the structure of the steel.

[0042] Furthermore, the specific steps of the cryogenic treatment are: placing the workpiece after the solution treatment at -196 to -150°C for 10 to 180 minutes, and then placing it in the air to heat it to room temperature.

[0043] From the above description, it can be seen that the appropriate temperature and holding time in cryogenic treatment enable complete transformation of martensite, while inhibiting the formation of reverse transformed austenite, precipitating ultrafine carbides on the martensite matrix, improving the uniformity of the structure, and ensuring that the steel obtains a full martensitic structure after cryogenic treatment.

[0044] Furthermore, the specific steps of the aging treatment are: placing the workpiece after deep cryogenic treatment in a vacuum environment, keeping it at 460-550° C. for 30-960 minutes, and then cooling it to room temperature.

[0045] From the above description, it can be seen that the appropriate temperature and holding time in the aging treatment allow carbides to precipitate, further improving the hardness, strength and toughness of the material.

[0046] Further, the volume ratio of MIM powder to binder is 1.30:1 to 1.85:1. Preferably, the volume ratio of MIM powder to binder is 1:57 to 1.70:1. More preferably, the volume ratio of MIM powder to binder is 1.59:1 to 1.65:1.

[0047] From the above description, it can be seen that the addition of binder can improve the rheological properties of the feed and ensure that the green body can be smoothly separated from the mold.

[0048] Furthermore, the adhesive comprises, by weight percentage, 80-90% of polyoxymethylene, 5-10% of polyethylene and 0-15% of a compatibilizer.

[0049] Furthermore, the adhesive is composed of the following components by weight: 80-90% of polyoxymethylene, 5-10% of polyethylene, 0-4% of paraffin and 3-10% of a compatibilizer.

[0050] Embodiment 1 of the present invention is:

[0051] A MIM forming process for 1800MPa ultra-high strength and high toughness steel comprises the following steps:

[0052] S1: Raw material selection, MIM powder is composed of the following metal powders in weight percentage: C 0.3%, Cr2.5%, Ni12.5%, Co 15.5%, Mo 1.8%, Mn 0.3%, Si 0.2%, S 0.002%, P 0.001% and the balance Fe, the particle size of MIN powder is ≤30μm;

[0053] The binder is composed of the following components: 87% polyoxymethylene, 8% polyethylene, 3% paraffin and the balance stearic acid.

[0054] S2: adding MIM powder and binder in a volume ratio of 1.60:1 into an internal mixer and kneading to obtain a feed material, and then granulating the feed material;

[0055] S3: The granulated feed material is injection molded into a green body through an injection molding machine and a mold; the injection temperature is 190° C., the screw speed is 60 r / min, and the injection pressure is 200 MPa.

[0056] S4: The green body is placed in a degreasing furnace and catalytic degreasing is performed using nitric acid; the temperature of the catalytic degreasing is 100°C, the time is 8h, and the acid flow rate is 4g / min.

[0057] S5: Place the green body after catalytic debinding in a sintering furnace for negative pressure debinding, introduce argon gas with a flow rate of 40L / min, increase the temperature in the sintering furnace from room temperature to 300℃ at a heating rate of 2℃ / min, and keep it warm for 60min; increase the temperature in the sintering furnace from 300℃ to 450℃ at a heating rate of 1.5℃ / min, and keep it warm for 60min; increase the temperature in the sintering furnace from 450℃ to 600℃ at a heating rate of 1℃ / min, and keep it warm for 60min to complete the thermal debinding.

[0058] S6. Maintain the pressure in the sintering furnace <10Pa, increase the temperature in the sintering furnace from 600°C to 1150°C at a heating rate of 4°C / min, and then keep it warm for 60 minutes to complete deoxidation and decarburization.

[0059] S7: Maintain the argon pressure in the sintering furnace at 20 kPa, increase the temperature in the sintering furnace from 1150°C to 1360°C at a heating rate of 5°C / min, then keep warm for 180 minutes, and then cool to room temperature to complete sintering and obtain a sintered part.

[0060] S8: Under vacuum conditions, the sintered part is kept at 1000°C for 60 minutes and then cooled to room temperature. The cooling medium is 800 kPa argon gas and the cooling rate is 300°C / min to complete the solution treatment.

[0061] S9: Place the workpiece after solution treatment in liquid nitrogen at -150°C, keep it warm for 60 minutes, take it out, and then place it in the air to heat it to room temperature to complete the deep cryogenic treatment.

[0062] S10: Under vacuum conditions, the workpiece after cryogenic treatment is kept at 480°C for 120 minutes, and then cooled to room temperature to complete the aging treatment to obtain ultra-high strength and high toughness steel parts.

[0063] Ultra-high strength and high toughness steel parts have a tensile strength of 2180MPa, a yield strength of 1850MPa, an elongation of 6% (test reference standard GB / T 228.1-2010), and a hardness of 57HRC.

[0064] Embodiment 2 of the present invention is:

[0065] A MIM forming process for 1800MPa ultra-high strength and high toughness steel comprises the following steps:

[0066] S1: Raw material selection. The MIM powder is composed of the following metal powders in weight percentage: C 0.15%, Cr 2.0%, Ni 11.5%, Co 17.0%, Mo 2.5%, Mn 0.1%, Si 0.3%, S 0.005%, P 0.005% and the balance Fe. The particle size of the MIM powder is ≤25μm.

[0067] The adhesive is composed of the following components: 90% polyoxymethylene, 7% polyethylene and the balance ethylene-vinyl acetate copolymer.

[0068] S2: MIM powder and binder are added into an internal mixer at a volume ratio of 1.85:1, and kneaded to obtain feed material, and then the feed material is crushed.

[0069] S3: The crushed feed material is injection molded into a green body through an injection molding machine and a mold; the injection temperature is 195° C., the screw speed is 80 r / min, and the injection pressure is 220 MPa.

[0070] S4: The green body is placed in a degreasing furnace and catalytic degreasing is performed using nitric acid; the temperature of the catalytic degreasing is 110°C, the time is 10 hours, and the acid flow rate is 2.5 g / min.

[0071] S5: Place the green body after catalytic debinding in a sintering furnace for negative pressure debinding, introduce nitrogen with a nitrogen flow rate of 50L / min, raise the temperature in the sintering furnace from room temperature to 300℃ at a heating rate of 5℃ / min, and keep it warm for 20min; raise the temperature in the sintering furnace from 300℃ to 450℃ at a heating rate of 1℃ / min, and keep it warm for 20min; raise the temperature in the sintering furnace from 450℃ to 800℃ at a heating rate of 0.5℃ / min, and keep it warm for 20min to complete the thermal debinding.

[0072] S6. Maintain the pressure in the sintering furnace at <10Pa, increase the temperature in the sintering furnace from 500°C to 1050°C at a heating rate of 1.5°C / min, and then keep it warm for 10 minutes to complete deoxidation and decarburization.

[0073] S7: Maintaining the argon pressure in the sintering furnace at 10 kPa, raising the temperature in the sintering furnace from 1050°C to 1340°C at a heating rate of 1.5°C / min, then keeping the temperature for 360 minutes, and then cooling to room temperature to complete the sintering and obtain a sintered part.

[0074] S8: In vacuum, the sintered part is kept at 1050°C for 60 minutes and then cooled to room temperature. The cooling medium is 400 kPa nitrogen and the cooling rate is 100°C / min to complete the solution treatment.

[0075] S9: Place the workpiece after solution treatment in liquid nitrogen at -196°C, keep it warm for 10 minutes, take it out, and then place it in the air to warm up to room temperature to complete the deep cryogenic treatment.

[0076] S10: In vacuum, the workpiece after cryogenic treatment is kept at 470°C for 240 minutes, and then cooled to room temperature to complete the aging treatment to obtain ultra-high strength and high toughness steel parts.

[0077] Ultra-high strength and high toughness steel parts have a tensile strength of 2260MPa, a yield strength of 1895MPa, an elongation of 5.5% (test reference standard GB / T 228.1-2010), and a hardness of 58HRC.

[0078] Embodiment 3 of the present invention is:

[0079] A MIM forming process for 1800MPa ultra-high strength and high toughness steel comprises the following steps:

[0080] S1: Raw material selection. MIM powder is composed of the following metal powders in weight percentage: C 0.6%, Cr 3.5%, Ni 11.0%, Co 14.0%, Mo 1.5%, Mn 1.0%, Si 0.02%, S 0.01%, P 0.01% and the balance Fe. The particle size of MIM powder is ≤20μm.

[0081] The adhesive consists of the following components: 90% polyoxymethylene, 5% polyethylene, 3% ethylene-vinyl acetate copolymer and 2% paraffin.

[0082] S2: Add MIM powder and binder in a volume ratio of 1.30:1 into an internal mixer and knead to obtain feed material, and then crush and granulate the feed material in sequence.

[0083] S3: The granulated feed material is injection molded into a green body through an injection molding machine and a mold; the injection temperature is 185° C., the screw speed is 50 r / min, and the injection pressure is 240 MPa.

[0084] S4: The green body is placed in a degreasing furnace and catalytic degreasing is performed using nitric acid; the temperature of the catalytic degreasing is 120°C, the time is 6 hours, and the acid flow rate is 3g / min.

[0085] S5: Place the green body after catalytic debinding in a sintering furnace for negative pressure debinding, introduce nitrogen with a flow rate of 30L / min, raise the temperature in the sintering furnace from room temperature to 300°C at a heating rate of 10°C / min, and keep it warm for 60 minutes; raise the temperature in the sintering furnace from 300°C to 450°C at a heating rate of 5°C / min, and keep it warm for 60 minutes; raise the temperature in the sintering furnace from 450°C to 800°C at a heating rate of 2°C / min, and keep it warm for 60 minutes to complete the thermal debinding.

[0086] S6. Maintain the pressure in the sintering furnace <10Pa, increase the temperature in the sintering furnace from 800°C to 950°C at a heating rate of 1°C / min, and then keep it warm for 240 minutes to complete deoxidation and decarburization.

[0087] S7: Maintaining the argon pressure in the sintering furnace at 20 kPa, raising the temperature in the sintering furnace from 900°C to 1350°C at a heating rate of 5°C / min, then keeping the temperature for 180 minutes, and then cooling to room temperature to complete the sintering and obtain a sintered part.

[0088] S8: In vacuum, the sintered part is kept at 1150°C for 30 minutes and then cooled to room temperature. The cooling medium is 1000 kPa argon gas and the cooling rate is 300°C / min to complete the solution treatment.

[0089] S9: Place the workpiece after solution treatment in liquid nitrogen at -150°C, keep it warm for 180 minutes, take it out, and then place it in the air to heat it to room temperature to complete the deep cryogenic treatment.

[0090] S10: In vacuum, the workpiece after cryogenic treatment is kept at 550°C for 30 minutes, and then cooled to room temperature to complete the aging treatment to obtain ultra-high strength and high toughness steel parts.

[0091] Ultra-high strength and high toughness steel parts have a tensile strength of 2230MPa, a yield strength of 1920MPa, an elongation of 6.0% (test reference standard GB / T 228.1-2010), and a hardness of 57HRC.

[0092] Embodiment 4 of the present invention is:

[0093] A MIM forming process for 1800MPa ultra-high strength and high toughness steel comprises the following steps:

[0094] S1: Raw material selection. MIM powder is composed of the following metal powders in weight percentage: C 0.0%, Cr 3.0%, Ni 14.0%, Co 16.5%, Mo 2.0%, Mn 0.05%, Si 1.0%, S 0.001%, P 0.001% and the balance Fe. The particle size of MIM powder is ≤50μm.

[0095] The binder is composed of the following components by weight: 86% of polyoxymethylene, 7% of polyethylene, 4% of zinc stearate, and 3% of paraffin.

[0096] S2: Add MIM powder and binder in a volume ratio of 1.70:1 into an internal mixer and knead to obtain feed material, and then crush the feed material.

[0097] S3: The crushed feed material is injection molded into a green body through an injection molding machine and a mold; the injection temperature is 195° C., the screw speed is 80 r / min, and the injection pressure is 220 MPa.

[0098] S4: The green body is placed in a degreasing furnace and catalytic degreasing is performed using nitric acid; the temperature of the catalytic degreasing is 110°C, the time is 10 hours, and the acid flow rate is 6 g / min.

[0099] S5: Place the green body after catalytic debinding in a sintering furnace for negative pressure debinding, introduce argon gas with a flow rate of 50L / min, and increase the temperature in the sintering furnace from room temperature to 350℃ at a heating rate of 0.1℃ / min; increase the temperature in the sintering furnace from 350℃ to 500℃ at a heating rate of 3℃ / min; increase the temperature in the sintering furnace from 500℃ to 800℃ at a heating rate of 0.1℃ / min to complete thermal debinding.

[0100] S6. Maintain the pressure in the sintering furnace at <10Pa, increase the temperature in the sintering furnace from 800°C to 900°C at a heating rate of 1°C / min, and then keep it warm for 10 minutes to complete deoxidation and decarburization.

[0101] S7: Maintain the argon pressure in the sintering furnace at 10 kPa, increase the temperature in the sintering furnace from 900°C to 1320°C at a heating rate of 2°C / min, then keep the temperature for 360 minutes, and then cool to room temperature to complete the sintering and obtain a sintered part.

[0102] S8: In vacuum, the sintered part is kept at 950°C for 180 min and then cooled to room temperature. The cooling medium is 100 kPa nitrogen and the cooling rate is 50°C / min to complete the solution treatment.

[0103] S9: Place the workpiece after solution treatment in liquid nitrogen at -180°C, keep it warm for 90 minutes, take it out, and then place it in the air to heat it to room temperature to complete the deep cryogenic treatment.

[0104] S10: In vacuum, the workpiece after cryogenic treatment is kept at 460°C for 960 minutes, and then cooled to room temperature to complete the aging treatment to obtain ultra-high strength and high toughness steel parts.

[0105] Ultra-high strength and high toughness steel parts have a tensile strength of 2165MPa, a yield strength of 1840MPa, an elongation of 7.3% (test reference standard GB / T 228.1-2010), and a hardness of 52HRC.

[0106] Embodiment 5 of the present invention is:

[0107] A MIM forming process for 1800MPa ultra-high strength and high toughness steel comprises the following steps:

[0108] S1: Raw material selection. MIM powder is composed of the following metal powders in weight percentage: C 0.2%, Cr2.8%, Ni13.0%, Co 16.0%, Mo 2.2%, Mn 0.05%, Si 0.05%, S 0.008%, P 0.002% and the balance Fe. The particle size of MIM powder is ≤20μm.

[0109] The binder is composed of the following components by weight percentage: 80% polyoxymethylene, 10% polyethylene, 4% ethylene-vinyl acetate copolymer, 4% stearic acid and 2% paraffin.

[0110] S2: MIM powder and binder are added into an internal mixer at a volume ratio of 1.59:1 and kneaded to obtain feed material, and then the feed material is crushed and granulated in sequence.

[0111] S3: The granulated feed material is injection molded into a green body through an injection molding machine and a mold; the injection temperature is 185° C., the screw speed is 50 r / min, and the injection pressure is 240 MPa.

[0112] S4: The green body is placed in a degreasing furnace and catalytic degreasing is performed using nitric acid; the temperature of the catalytic degreasing is 120°C, the time is 6 hours, and the acid flow rate is 3g / min.

[0113] S5: Place the green body after catalytic debinding in a sintering furnace for negative pressure debinding, introduce argon gas with a flow rate of 30L / min, increase the temperature in the sintering furnace from room temperature to 250℃ at a heating rate of 10℃ / min, and keep it warm for 180min; increase the temperature in the sintering furnace from 250℃ to 400℃ at a heating rate of 8℃ / min, and keep it warm for 180min; increase the temperature in the sintering furnace from 400℃ to 550℃ at a heating rate of 3℃ / min, and keep it warm for 180min to complete the thermal debinding.

[0114] S6. Maintain the pressure in the sintering furnace <10Pa, increase the temperature in the sintering furnace from 550°C to 1200°C at a heating rate of 1°C / min, and then keep it warm for 240 minutes to complete deoxidation and decarburization.

[0115] S7: Maintain the argon pressure in the sintering furnace at 50 kPa, increase the temperature in the sintering furnace from 1200°C to 1380°C at a heating rate of 1°C / min, then keep warm for 30 minutes, and then cool to room temperature to complete sintering and obtain a sintered part.

[0116] S8: In vacuum, the sintered part is kept at 1150°C for 10 min and then cooled to room temperature. The cooling medium is 1000 kPa argon gas and the cooling rate is 300°C / min to complete the solution treatment.

[0117] S9: Place the workpiece after solution treatment in liquid nitrogen at -170°C, keep it warm for 180 minutes, take it out, and then place it in the air to heat it to room temperature to complete the deep cryogenic treatment.

[0118] S10: In vacuum, the workpiece after cryogenic treatment is kept at 550°C for 30 minutes, and then cooled to room temperature to complete the aging treatment to obtain ultra-high strength and high toughness steel parts.

[0119] Ultra-high strength and high toughness steel parts have a tensile strength of 2205MPa, a yield strength of 1875MPa, an elongation of 5.2% (test reference standard GB / T 228.1-2010), and a hardness of 55.8HRC.

[0120] Comparative Example 1 of the present invention is:

[0121] The difference between Comparative Example 1 and Example 1 is that the weight percentage of Ni in the MIM powder is 10%, and the weight percentage of Co is 18%. The obtained parts have a tensile strength of 2010MPa, a yield strength of 1850MPa, an elongation of 1.5% (test reference standard GB / T 228.1-2010), and a hardness of 59HRC.

[0122] Comparative Example 2 of the present invention is:

[0123] The difference between Comparative Example 2 and Example 1 is that the weight percentage of Ni in the MIM powder is 18%, and the weight percentage of Co is 10%. The obtained parts have a tensile strength of 930 MPa, a yield strength of 650 MPa, an elongation of 25.0% (test reference standard GB / T 228.1-2010), and a hardness of 30 HRC.

[0124] In summary, the MIM forming process of ultra-high strength and high toughness steel parts provided by the present invention adopts a specific ratio of Co and Ni metals to prepare a green billet, and then sequentially undergoes catalytic degreasing, hot degreasing, deoxidation and decarburization, sintering, solid solution treatment, deep cryogenic treatment and aging treatment to obtain an ultra-high strength and high toughness steel with a yield strength ≥1800MPa, an elongation ≥5%, and a hardness of 52 to 58HRC. It can meet the requirements of 3C, tools, automobiles, aerospace and other industries for ultra-high strength, high toughness and wear-resistant parts, and has the advantages of high production efficiency, low cost, and good dimensional consistency.

[0125] Among them, solution treatment, cryogenic treatment and aging treatment are the key steps to form martensite, martensitic phase transformation and carbide precipitation; solution treatment can ensure that the components in the alloy can be evenly dissolved into the matrix to form a uniform solid solution, which has the effect of improving elongation. Cryogenic treatment allows the martensitic transformation to be complete, while inhibiting the formation of reverse transformed austenite, precipitating ultrafine carbides on the martensitic matrix, improving the uniformity of the structure, and ensuring that the steel obtains a full martensitic structure after cryogenic treatment. Aging treatment allows carbides to precipitate, further improving the hardness, strength and toughness of the material.

[0126] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the specification of the present invention, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A MIM forming process for 1800MPa ultra-high strength and high toughness steel, characterized in that: The following steps are involved: S1: kneading MIM powder and binder to obtain feed material, and then crushing and / or granulating the feed material; S2: injection molding the crushed and / or granulated feed into a green body; S3: catalytically debinding the green body; S4: The green body after catalytic debinding is subjected to thermal debinding, deoxidation and decarburization and sintering in an inert gas atmosphere of 0 to 50 kPa in sequence to obtain a sintered part; S5: The sintered parts are subjected to solution treatment, cryogenic treatment and aging treatment in sequence to obtain ultra-high strength and high toughness steel; The specific steps of the solution treatment are: placing the sintered part in a vacuum environment, keeping it at 950-1150°C for 10-180 minutes, and then cooling it to room temperature, the cooling medium is nitrogen and / or argon, the cooling rate is ≥50°C / min, and the pressure of the cooling medium is 100-1000kPa; The specific steps of the deep cryogenic treatment are: placing the workpiece after the solution treatment at -196 to -150°C for 10 to 180 minutes, and then placing it in the air to heat it to room temperature; The specific steps of the aging treatment are: placing the workpiece after deep cryogenic treatment in a vacuum environment, keeping the temperature at 460-550° C. for 30-960 min, and then cooling to room temperature; The MIM powder is composed of the following powders in weight percentage: C 0.1-0.4%, Cr 2.0-3.5%, Ni 11.0-13.0%, Co 15.0-17.0%, Mo 1.5-2.0%, impurities 0-2.02%, and the balance of iron; the particle size of the MIM powder is ≤25 μm.

2. The MIM forming process of 1800MPa ultra-high strength and high toughness steel according to claim 1, characterized in that: The specific steps of the thermal degreasing are: raising the ambient temperature from room temperature to 250-350°C at a heating rate of 0.1-10°C / min, and keeping it warm for 0-180min; continuing to raise the ambient temperature to 400-500°C at a heating rate of 0.1-10°C / min, and keeping it warm for 0-180min; continuing to raise the ambient temperature to 550-800°C at a heating rate of 0.1-10°C / min, and keeping it warm for 0-180min.

3. The MIM forming process of 1800MPa grade ultra-high strength and high toughness steel according to claim 1, characterized in that: The specific steps of deoxidation and decarburization are: controlling the gas pressure in the furnace to be less than 10Pa, raising the ambient temperature from 500-800°C to 900-1200°C at a heating rate of 0.1-8°C / min, and then keeping the temperature for 10-240 minutes.

4. The MIM forming process of 1800MPa grade ultra-high strength and high toughness steel according to claim 1, characterized in that: The specific steps of sintering are: raising the ambient temperature from 900-1200°C to 1320-1380°C at a heating rate of 0.1-10°C / min, then keeping the temperature for 30-360min, and cooling to room temperature to obtain a sintered part.

5. The MIM forming process of 1800MPa grade ultra-high strength and high toughness steel according to claim 1, characterized in that: The volume ratio of the MIM powder to the binder is 1.30:1 to 1.85:1.

Citation Information

Cited By

  • Ultrahigh-strength high-toughness steel powder injection molding process

    CN121082891A