A protective film for laser cutting of optical lenses and preparation method thereof

By using a protective film including a release layer, a functional PE substrate layer and a rubber-based pressure-sensitive adhesive layer in laser cutting of optical lenses, the problems of cutting degumming and floating film are solved, and high light transmittance and clear cutting marks are achieved. display, ensuring product quality.

CN115746736BActive Publication Date: 2024-10-29XIANGYANG SUNVALOR AEROSPACE FILMS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211573876.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-08
Publication Date
2024-10-29
Estimated Expiration
2042-12-08

AI Technical Summary

Technical Problem

Existing optical glass cutting protective films are prone to cutting degumming and film drifting during the laser cutting process, and the transmittance is not enough to clearly display cutting marks, making it difficult to meet the needs of optical lenses.

Method used

A protective film including a release layer, a functional PE base material layer and a rubber-based pressure-sensitive adhesive layer is used. The functional PE base material layer is composed of low density polyethylene, linear low density polyethylene, fillers and functional masterbatch. The rubber-based pressure-sensitive adhesive layer is composed of butadiene rubber, tackifying resin and antioxidant. Through a specific hierarchical structure, material ratio and preparation method, the light transmittance and degumming resistance of the film are ensured.

Benefits of technology

It achieves no degumming and no floating film during the laser cutting process, and improves the transmittance to ensure that the cutting mark is clearly visible, enhances the viscosity and wettability of the film, and avoids contamination and product quality problems during the cutting process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115746736B_ABST
    Figure CN115746736B_ABST
Patent Text Reader

Abstract

The present invention proposes a protective film for laser cutting of optical lenses and a preparation method thereof, wherein the protective film comprises a release layer, a functional PE substrate layer, a primer layer and a rubber-based pressure-sensitive adhesive layer from top to bottom; the preparation materials of the functional PE substrate layer include: low-density polyethylene, linear low-density polyethylene, fillers and functional masterbatches; the functional masterbatches include one or more combinations of PMMA powder, alumina and ultrafine carbon black, and the fillers are nano-scale inorganic fillers, including one or more combinations of barium sulfate, calcium sulfate and calcium carbonate. The protective film of the present invention has a high transmittance, and the cutting mark can be clearly seen; at the same time, it can effectively absorb the energy generated by the laser, so that the protective film is quickly melted during the film cutting process, and the slag is taken away by the strong wind pressure, which effectively solves the product quality problems caused by the phenomenon of debonding and film floating during cutting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of protective films, and in particular to a protective film for laser cutting of optical lenses and a preparation method thereof. Background Art

[0002] With the rapid development of laser cutting technology, the processing technology of optical glass has successfully achieved great progress from mechanical cutting to low-power picosecond laser cutting. Since the surface of optical glass must maintain absolute cleanliness, there is a risk of cutting debris falling and contaminating the lens even in an ultra-clean processing environment. Coating cutting has become the simplest and most effective solution to the above problem.

[0003] The commonly used optical glass cutting protective film is a self-adhesive film based on PE substrate. Under high-temperature laser cutting and strong wind pressure, it is easy to cause debonding and film floating during cutting, causing product quality problems. In addition, during the cutting process, the laser cutting machine will position and cut according to the coating mark in the optical glass, so there are certain requirements for the transmittance of the protective film. The invention patent with patent number CN112980346A provides an ultra-high transmittance protective film, but the protective film is suitable for process protection of electronic products and not suitable for laser film cutting of optical lenses. Therefore, a lens protective film with high transmittance and can be used for laser cutting is needed. Summary of the invention

[0004] In view of this, the present invention proposes an optical lens protective film which has high light transmittance and does not debond or float when the optical lens is laser cut.

[0005] The technical solution of the present invention is implemented as follows: on the one hand, the present invention provides a protective film for laser cutting of optical lenses, wherein the protective film comprises a release layer, a functional PE substrate layer, a primer layer and a rubber-based pressure-sensitive adhesive layer from top to bottom; the preparation materials of the functional PE substrate layer include: low-density polyethylene, linear low-density polyethylene, fillers and functional masterbatches; the functional masterbatches include one or more combinations of PMMA powder, alumina and ultrafine carbon black, and the fillers are nano-scale inorganic fillers, including one or more combinations of barium sulfate, calcium sulfate and calcium carbonate.

[0006] On the basis of the above technical solution, preferably, the functional PE substrate layer includes an outer layer, a middle layer and an inner layer from top to bottom, the outer layer is close to the release layer, and the inner layer is close to the primer layer;

[0007] Calculated based on the mass percentage of 100%, the outer layer is made of the following raw materials: 49%-70% low-density polyethylene, 29.5%-50% linear low-density polyethylene and 0.5%-1% calcium stearate;

[0008] Calculated based on the mass percentage of 100%, the middle layer is made of the following raw materials: 50%-70% of linear low-density polyethylene, 10-20% of functional masterbatch and 20-30% of modified masterbatch;

[0009] Calculated by mass percentage as 100%, the modified masterbatch is made of the following raw materials: 12%-14% of filler, 1%-3% of surfactant and 83%-87% of linear low-density polyethylene;

[0010] Calculated based on the mass percentage of 100%, the functional masterbatch is made of the following raw materials: 0.5%-1% functional masterbatch, 1-2% surfactant and 97%-98.5% linear low-density polyethylene;

[0011] Calculated based on the mass percentage of 100%, the inner layer is made of the following raw materials: 30%-69.7% of low-density polyethylene, 30%-69.3% of linear low-density polyethylene and 0.3%-0.7% of calcium stearate.

[0012] On the basis of the above technical solution, preferably, the surfactant is one or a mixture of white oil, polyethylene wax, stearic acid and paraffin.

[0013] Based on the above technical solution, preferably, the release agent of the release layer is one or more combinations of SYL-OFF7955, EPOMIN, Berkeley UCB2000 and RP-20; the primer of the base coat layer is one or two combinations of 3M94 primer and 3Mac77 primer.

[0014] On the basis of the above technical solution, preferably, calculated by mass percentage as 100%, the rubber-based pressure-sensitive adhesive layer is made of the following raw materials: 10%-20% rubber matrix, 10%-15% tackifying resin, 0.1%-0.5% antioxidant and 64.5%-79.9% solvent.

[0015] On the basis of the above technical scheme, preferably, the base rubber is one or a mixture of butadiene rubber, styrene-butadiene rubber, synthetic isoprene rubber and natural rubber; the tackifying resin is one or a mixture of rosin glycerol ester resin, rosin pentaerythritol ester resin, rosin phenolic ester resin, α-terpene resin, β-terpene resin, C5 hydrogenated petroleum resin, C9 hydrogenated petroleum resin and coumarone resin; the antioxidant is one or a mixture of antioxidant BHT, antioxidant DBH, antioxidant DNP, antioxidant RD, antioxidant MB, antioxidant MMB, antioxidant 2246, antioxidant 4010NA, antioxidant 4020 and antioxidant 1076; the solvent is one or a mixture of toluene, xylene, gasoline, n-hexane, cyclohexane, pentane and heptane.

[0016] On the basis of the above technical scheme, preferably, the preparation method of the pressure-sensitive adhesive of the rubber-based pressure-sensitive adhesive layer is: adjust the temperature of the dissolving kettle to 50-60°C, the stirring frequency is 30-50HZ, the solvent is added into the dissolving kettle, and then the tackifying resin, the antioxidant, and the base rubber are sequentially added into the kettle and stirred to dissolve, and the stirring and dissolving is continued for 10-12 hours, and then the material is filtered out to obtain the pressure-sensitive adhesive.

[0017] On the other hand, the present invention provides a method for preparing a protective film for laser cutting of optical lenses, comprising the following steps:

[0018] S1, using a film blowing machine to prepare a PE base film by three-layer co-extrusion to obtain a functional PE base layer;

[0019] S2, respectively applying a release agent and a primer to the outer layer and the inner layer of the functional PE substrate layer by means of a screen roller coating, and drying to obtain a semi-finished product having a release layer, a functional PE substrate layer and a primer layer;

[0020] S3, a layer of rubber-based pressure-sensitive adhesive is roller-coated on the base coating layer, and after drying, a protective film having a release layer, a functional PE substrate layer, a base coating layer and a rubber-based pressure-sensitive adhesive layer is prepared.

[0021] Based on the above technical solution, preferably, the thickness of the release layer is 0.05-0.1 μm, the thickness of the functional PE substrate layer is 80-100 μm, the thickness ratio of the outer layer: middle layer: inner layer is 1:1:1, the thickness of the primer layer is 0.1-0.5 μm, and the thickness of the rubber-based pressure-sensitive adhesive layer is 5-15 μm.

[0022] On the basis of the above technical solution, preferably, in step S1, the blown film extrusion temperatures are: 175-180°C for the outer layer, 140-175°C for the middle layer, and 175-180°C for the inner layer.

[0023] The protective film for laser cutting of optical lenses and the preparation method of the present invention have the following beneficial effects compared with the prior art:

[0024] (1) The functional PE substrate layer of the present invention has the function of absorbing infrared light, which can effectively absorb the energy generated by the laser, so that the protective film can be quickly melted during the film cutting process, and the slag is taken away by the strong wind pressure; on the other hand, the transmittance of the film is improved, and the cutting mark can be clearly seen.

[0025] (2) The primer layer of the present invention improves the bonding strength between the rubber-type pressure-sensitive adhesive and the PE functional film substrate layer, thereby preventing the adhesive layer from falling off the lens surface and contaminating the lens product.

[0026] (3) Since the rubber molecules of rubber-type pressure-sensitive adhesive have large molecular weight and long molecular chain, the colloid is soft and has good adhesion and wettability. During the process of rolling without release paper, it is easy to be unable to unwind. Therefore, the present invention coats the release agent on the outer surface of the base film to facilitate the unwinding of the protective film.

[0027] (4) The rubber-based pressure-sensitive adhesive layer of the present invention has the advantages of good adhesion, no debonding and good wettability. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 It is a structural diagram of the protective film of the present invention.

[0030] In the figure, 1-release layer, 2-functional PE substrate layer, 21-outer layer, 22-middle layer, 23-inner layer, 3-primer coating layer, 4-rubber-based pressure-sensitive adhesive layer. DETAILED DESCRIPTION

[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] The reagents and materials used in the present invention are purchased from the market. The ultrafine carbon black particle size is 5-100nm, and the total pore volume is 0.5-1.8cm 3 / g, the particle size of nano-scale barium sulfate, calcium sulfate and calcium carbonate is <0.3μm, the linear low-density polyethylene is Sinopec EGF-35B material, and the low-density polyethylene is ExxonMobil LD-158 Series LDPE material.

[0033] Embodiment 1

[0034] The protective film of this embodiment includes, from top to bottom, a release layer, a functional PE substrate layer, a primer layer, and a rubber-based pressure-sensitive adhesive layer;

[0035] The release agent of the release layer is obtained by mixing 10g SYL-OFF7955 and 20g EPOMIN.

[0036] The functional PE substrate layer includes an outer layer, a middle layer and an inner layer from top to bottom, the outer layer is close to the release layer, and the inner layer is close to the primer layer.

[0037] The outer layer is prepared by blending 49 g of low-density polyethylene, 50 g of linear low-density polyethylene and 1 g of calcium stearate and extruding and granulating using a twin-screw extruder.

[0038] The middle layer is prepared by blending 50g of linear low-density polyethylene, 20g of functional masterbatch and 30g of modified masterbatch, and extruding and granulating using a twin-screw extruder. The modified masterbatch is prepared by blending 12g of nano-scale barium sulfate, 0.5g of white oil, 0.5g of polyethylene wax, and 87g of linear low-density polyethylene, and extruding and granulating using a twin-screw extruder. The functional masterbatch is prepared by blending 0.5g of PMMA powder, 1g of white oil and 98.5g of linear low-density polyethylene, and extruding and granulating using a twin-screw extruder.

[0039] The inner layer is prepared by blending 30 g of low-density polyethylene, 69.3 g of linear low-density polyethylene and 0.7 g of calcium stearate and extruding and granulating using a twin-screw extruder.

[0040] The primer of the bottom coating layer is 3M94 primer.

[0041] The preparation method of the rubber-based pressure-sensitive adhesive of the rubber-based pressure-sensitive adhesive layer is as follows: the temperature of the dissolving kettle is adjusted to 50°C, the stirring frequency is 40HZ, 79.9g of toluene solvent is added into the dissolving kettle, and then 5g of rosin glycerol ester resin, 5g of α-terpene resin, 0.1g of antioxidant BHT, and 10g of butadiene rubber are added into the kettle in sequence and stirred to dissolve, and stirring and dissolving is continued for 10 hours, and the material is filtered to obtain the rubber-based pressure-sensitive adhesive.

[0042] The method for preparing a protective film comprises the following steps:

[0043] S1, using a blown film machine to co-extrude a PE base film to obtain a functional PE base layer, the blown film extrusion temperatures are: 175°C for the outer layer, 140°C for the middle layer, and 175°C for the inner layer;

[0044] S2, respectively applying a release agent and a primer to the outer layer and the inner layer of the functional PE substrate layer by means of a screen roller coating, and drying to obtain a semi-finished product having a release layer, a functional PE substrate layer and a primer layer;

[0045] S3, a layer of rubber-based pressure-sensitive adhesive is roller-coated on the base coating layer, and after drying, a protective film having a release layer, a functional PE substrate layer, a base coating layer and a rubber-based pressure-sensitive adhesive layer is prepared.

[0046] The total thickness of the protective film is 86.15μm, of which the release layer thickness is 0.05μm, the thickness of the functional PE substrate layer is 81μm, the thickness of the outer layer, middle layer and inner layer are all 27μm, the thickness of the primer layer is 0.1μm, and the thickness of the rubber-based pressure-sensitive adhesive layer is 5μm.

[0047] Embodiment 2

[0048] The protective film of this embodiment includes, from top to bottom, a release layer, a functional PE substrate layer, a primer layer, and a rubber-based pressure-sensitive adhesive layer;

[0049] The release agent of the release layer is obtained by mixing 10g of Berkeley UCB2000 and 10g of RP-20.

[0050] The functional PE substrate layer includes an outer layer, a middle layer and an inner layer from top to bottom, the outer layer is close to the release layer, and the inner layer is close to the primer layer;

[0051] The outer layer is prepared by blending 64.2 g of low-density polyethylene, 35 g of linear low-density polyethylene and 0.8 g of calcium stearate and extruding and granulating using a twin-screw extruder.

[0052] The middle layer is prepared by blending 60g of linear low-density polyethylene, 15g of functional masterbatch and 25g of modified masterbatch, and extruding and granulating them using a twin-screw extruder. The modified masterbatch is prepared by blending 13g of nano-scale calcium sulfate, 2g of polyethylene wax and 85g of linear low-density polyethylene, and extruding and granulating them using a twin-screw extruder. The functional masterbatch is prepared by blending 0.6g of aluminum oxide, 1.5g of stearic acid and 97.9g of linear low-density polyethylene, and extruding and granulating them using a twin-screw extruder.

[0053] The inner layer is prepared by blending 50 g of low-density polyethylene, 49.5 g of linear low-density polyethylene and 0.5 g of calcium stearate and extruding and granulating using a twin-screw extruder.

[0054] The primer of the bottom coating layer is 3Mac77 primer.

[0055] The preparation method of the rubber-based pressure-sensitive adhesive of the rubber-based pressure-sensitive adhesive layer is as follows: the temperature of the dissolving kettle is adjusted to 50°C, the stirring frequency is 30HZ, 30g of xylene and 40g of gasoline are added into the dissolving kettle, and then 10g of rosin phenolic ester resin, 3g of C9 hydrogenated petroleum resin, 0.3g of antioxidant 4010NA, 12g of synthetic isoprene rubber and 4.7g of natural rubber are added into the kettle in sequence and stirred to dissolve, and stirring and dissolving is continued for 11 hours, and the material is filtered to obtain the product.

[0056] The method for preparing a protective film comprises the following steps:

[0057] S1, using a blown film machine to co-extrude a PE base film to obtain a functional PE base layer, the blown film extrusion temperatures are: 180°C for the outer layer, 150°C for the middle layer, and 180°C for the inner layer;

[0058] S2, respectively applying a release agent and a primer to the outer layer and the inner layer of the functional PE substrate layer by means of a screen roller coating, and drying to obtain a semi-finished product having a release layer, a functional PE substrate layer and a primer layer;

[0059] S3, a layer of rubber-based pressure-sensitive adhesive is roller-coated on the base coating layer, and after drying, a protective film having a release layer, a functional PE substrate layer, a base coating layer and a rubber-based pressure-sensitive adhesive layer is prepared.

[0060] The total thickness of the protective film is 100.38μm, of which the release layer thickness is 0.08μm, the thickness of the functional PE substrate layer is 90μm, the thickness of the outer layer, middle layer and inner layer are all 30μm, the thickness of the primer layer is 0.3μm, and the thickness of the rubber-based pressure-sensitive adhesive layer is 10μm.

[0061] Embodiment 3

[0062] The protective film of this embodiment includes, from top to bottom, a release layer, a functional PE substrate layer, a primer layer, and a rubber-based pressure-sensitive adhesive layer;

[0063] The release agent of the release layer is obtained by mixing 10g SYL-OFF7955 and 10g RP-20.

[0064] The functional PE substrate layer includes an outer layer, a middle layer and an inner layer from top to bottom, the outer layer is close to the release layer, and the inner layer is close to the primer layer.

[0065] The outer layer is prepared by blending 59.2 g of low-density polyethylene, 40 g of linear low-density polyethylene and 0.8 g of calcium stearate and extruding and granulating using a twin-screw extruder.

[0066] The middle layer is prepared by blending 52g of linear low-density polyethylene, 18g of functional masterbatch and 30g of modified masterbatch, and extruding and granulating using a twin-screw extruder. The modified masterbatch is prepared by blending 13% nano-scale calcium carbonate, 1g of white oil, 1.5g of paraffin and 84.5g of linear low-density polyethylene, and extruding and granulating using a twin-screw extruder. The functional masterbatch is prepared by blending 0.8g of ultrafine carbon black, 1g of white oil, 1g of stearic acid and 97.2g of linear low-density polyethylene, and extruding and granulating using a twin-screw extruder.

[0067] The inner layer is prepared by blending 69.4 g of low-density polyethylene, 30 g of linear low-density polyethylene and 0.6 g of calcium stearate and extruding and granulating using a twin-screw extruder.

[0068] The primer of the bottom coating layer is 3M94 primer.

[0069] The preparation method of the rubber-based pressure-sensitive adhesive of the rubber-based pressure-sensitive adhesive layer is as follows: adjust the temperature of the dissolving kettle to 50°C, the stirring frequency to 50HZ, put 35g of n-hexane and 33g of xylene into the dissolving kettle, and then put 10g of coumarone resin, 5g of β-terpene resin, 0.4g of antioxidant 1076, 10g of butadiene rubber, and 6.6g of styrene-butadiene rubber into the kettle in turn and stir to dissolve, continue stirring and dissolving for 12h, and filter the material to obtain the product.

[0070] The method for preparing a protective film comprises the following steps:

[0071] S1, using a blown film machine to prepare a PE base film by three-layer co-extrusion to obtain a functional PE base layer, the blown film extrusion temperatures are: 178°C for the outer layer, 160°C for the middle layer, and 178°C for the inner layer;

[0072] S2, respectively applying a release agent and a primer to the outer layer and the inner layer of the functional PE substrate layer by means of a screen roller coating, and drying to obtain a semi-finished product having a release layer, a functional PE substrate layer and a primer layer;

[0073] S3, a layer of rubber-based pressure-sensitive adhesive is roller-coated on the base coating layer, and after drying, a protective film having a release layer, a functional PE substrate layer, a base coating layer and a rubber-based pressure-sensitive adhesive layer is prepared.

[0074] The total thickness of the protective film is 109.48μm, the thickness of the release layer is 0.08μm, the thickness of the functional PE substrate layer is 96m, the thickness of the outer layer, middle layer and inner layer are all 32μm, the thickness of the primer layer is 0.4μm, and the thickness of the rubber-based pressure-sensitive adhesive layer is 13μm.

[0075] Embodiment 4

[0076] The protective film of this embodiment includes, from top to bottom, a release layer, a functional PE substrate layer, a primer layer, and a rubber-based pressure-sensitive adhesive layer;

[0077] The release agent of the release layer is a mixture of 10g SYL-OFF7955, 10g Berkeley UCB2000 and 10g RP-20.

[0078] The functional PE substrate layer includes an outer layer, a middle layer and an inner layer from top to bottom, the outer layer is close to the release layer, and the inner layer is close to the primer layer;

[0079] The outer layer is made of the following raw materials: 70 g of low-density polyethylene, 29.5 g of linear low-density polyethylene and 0.5 g of calcium stearate are blended and prepared by extrusion granulation using a twin-screw extruder.

[0080] The middle layer is made of the following raw materials: 70g of linear low-density polyethylene, 10g of functional masterbatch and 30g of modified masterbatch are blended and prepared by extrusion granulation using a twin-screw extruder.

[0081] The modified masterbatch is made of the following raw materials: 10g of nano-scale barium sulfate, 4g of nano-scale calcium sulfate, 1g of white oil, 2g of polyethylene wax and 83g of linear low-density polyethylene are blended and prepared by extrusion granulation using a twin-screw extruder.

[0082] The functional masterbatch is made of the following raw materials: 1g PMMA powder, 2g polyethylene wax and 97g linear low-density polyethylene are blended and prepared by extrusion granulation using a twin-screw extruder.

[0083] The inner layer is made of the following raw materials: 69.7 g of low-density polyethylene, 30 g of linear low-density polyethylene and 0.3 g of calcium stearate are blended and prepared by extrusion granulation using a twin-screw extruder.

[0084] The primer of the bottom coating layer is a mixture of 10g 3M94 primer and 10g 3Mac77 primer.

[0085] The preparation method of the rubber-based pressure-sensitive adhesive of the rubber-based pressure-sensitive adhesive layer is as follows: adjust the temperature of the dissolving kettle to 60°C, the stirring frequency to 50HZ, put 30g toluene and 49.9g heptane into the dissolving kettle, and then put 5g C9 hydrogenated petroleum resin, 5g α-terpene resin, 0.1g antioxidant 2246, 3g styrene-butadiene rubber, and 7g natural rubber into the kettle in turn and stir to dissolve, continue stirring and dissolving for 12h, and filter the material.

[0086] The method for preparing a protective film comprises the following steps:

[0087] S1, using a blown film machine to prepare a PE base film by three-layer co-extrusion to obtain a functional PE base layer, the blown film extrusion temperatures are: 180°C for the outer layer, 175°C for the middle layer, and 180°C for the inner layer;

[0088] S2, respectively applying a release agent and a primer to the outer layer and the inner layer of the functional PE substrate layer by means of a screen roller coating, and drying to obtain a semi-finished product having a release layer, a functional PE substrate layer and a primer layer;

[0089] S3, a layer of rubber-based pressure-sensitive adhesive is roller-coated on the base coating layer, and after drying, a protective film having a release layer, a functional PE substrate layer, a base coating layer and a rubber-based pressure-sensitive adhesive layer is prepared.

[0090] The total thickness of the protective film is 115.6μm, the thickness of the release layer is 0.1μm, the thickness of the functional PE substrate layer is 100μm, the thickness ratio of the outer layer: middle layer: inner layer is 1:1:1, the thickness of the primer layer is 0.5μm, and the thickness of the rubber-based pressure-sensitive adhesive layer is 15μm.

[0091] Comparative Example 1

[0092] The difference between Comparative Example 1 and Example 1 is that the middle layer of the functional PE substrate layer does not contain functional masterbatch, and the rest of the parts are the same.

[0093] Comparative Example 2

[0094] The difference between Comparative Example 2 and Example 1 is that the middle layer of the functional PE substrate layer does not contain modified masterbatch, and the rest of the parts are the same.

[0095] Comparative Example 3

[0096] The difference between Comparative Example 3 and Example 1 is that the middle layer of the functional PE substrate layer does not contain functional masterbatch and modified masterbatch, and the rest are the same.

[0097] The protective films prepared in the embodiments and comparative examples are used for laser cutting of optical glass lenses. The bottom rubber-based pressure-sensitive adhesive layer of the protective film is attached to the lens surface according to conventional technology, and laser cutting is performed according to conventional technical schemes and technical parameters; wherein the laser irradiation conditions are: wavelength of 355nm, repetition frequency of 100kHz, average power of 7W, irradiation times of 5 times / 1 line, pulse width of 50ns, focal point of ellipse (major axis of 100μm, minor axis of 10μm); laser cutting speed of 100mm / second.

[0098] The transmittance, peel strength and properties of the protective film under high temperature and high humidity conditions (70°C, 95%, 48h) and after being placed outdoors for 180 days were tested. The results are shown in Table 1. The laser cutting properties are shown in Table 2.

[0099] Table 1 Characteristics of protective film

[0100]

[0101] As shown in Table 1, the protective film without modified masterbatch and functional masterbatch has low permeability and peel strength, and is not resistant to high temperature, high humidity and aging.

[0102] Table 2 Status of protective film during laser cutting

[0103] Laser Cutting Embodiment 1 Clear marking, no debonding, no film floating Embodiment 2 Clear marking, no debonding, no film floating Embodiment 3 Clear marking, no debonding, no film floating Embodiment 4 Clear marking, no debonding, no film floating Comparative Example 1 The mark is not clear and the film is not cut Comparative Example 2 Clear markings and slag residue after film cutting Comparative Example 3 The mark is not clear, the basement membrane is soft and not cut off

[0104] As shown in Table 2, the protective film without modified masterbatch and functional masterbatch has problems such as low transmittance, unclear marking, soft base film that is difficult to cut, or film cut with residue when laser cutting.

[0105] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A protective film for laser cutting of optical lenses, characterized in that: The protective film includes a release layer, a functional PE substrate layer, a primer layer and a rubber-based pressure-sensitive adhesive layer from top to bottom; the release layer has a thickness of 0.05-0.1 μm, the functional PE substrate layer has a thickness of 80-100 μm, the primer layer has a thickness of 0.1-0.5 μm, and the rubber-based pressure-sensitive adhesive layer has a thickness of 5-15 μm; The preparation materials of the functional PE substrate layer include: low-density polyethylene, linear low-density polyethylene, filler and functional masterbatch; The functional masterbatch includes one or more combinations of PMMA powder, alumina and ultrafine carbon black, and the filler is a nano-scale inorganic filler, including one or more combinations of barium sulfate, calcium sulfate and calcium carbonate; The functional PE substrate layer includes an outer layer, a middle layer and an inner layer from top to bottom, the outer layer is close to the release layer, and the inner layer is close to the primer layer; the thickness ratio of the outer layer: the middle layer: the inner layer is 1:1:1; Calculated based on the mass percentage of 100%, the outer layer is made of the following raw materials: 49%-70% low-density polyethylene, 29.5%-50% linear low-density polyethylene and 0.5%-1% calcium stearate; Calculated based on the mass percentage of 100%, the middle layer is made of the following raw materials: 50%-70% of linear low-density polyethylene, 10-20% of functional masterbatch and 20-30% of modified masterbatch; Calculated by mass percentage as 100%, the modified masterbatch is made of the following raw materials: 12%-14% of filler, 1%-3% of surfactant and 83%-87% of linear low-density polyethylene; Calculated based on the mass percentage of 100%, the functional masterbatch is made of the following raw materials: 0.5%-1% functional masterbatch, 1-2% surfactant and 97%-98.5% linear low-density polyethylene; Calculated based on the mass percentage of 100%, the inner layer is made of the following raw materials: 30%-69.7% of low-density polyethylene, 30%-69.3% of linear low-density polyethylene and 0.3%-0.7% of calcium stearate.

2. A protective film for laser cutting of optical lenses as claimed in claim 1, characterized in that: The surfactant is one or a mixture of white oil, polyethylene wax, stearic acid and paraffin.

3. A protective film for laser cutting of optical lenses as claimed in claim 1, characterized in that: The release agent of the release layer is one or more combinations of SYL-OFF7955, EPOMIN, Berkeley UCB2000 and RP-20; the primer of the base coat is one or a combination of 3M94 primer and 3Mac77 primer.

4. The protective film for laser cutting of optical lenses according to claim 1, characterized in that: Calculated based on 100% by mass, the rubber-based pressure-sensitive adhesive layer is made of the following raw materials: 10%-20% of a rubber matrix, 10%-15% of a tackifying resin, 0.1%-0.5% of an antioxidant and 64.5%-79.9% of a solvent.

5. A protective film for laser cutting of optical lenses as claimed in claim 4, characterized in that: The rubber matrix is ​​one or a mixture of butadiene rubber, styrene-butadiene rubber, synthetic isoprene rubber and natural rubber; the tackifying resin is one or a mixture of rosin glycerol ester resin, rosin pentaerythritol ester resin, rosin phenolic ester resin, α-terpene resin, β-terpene resin, C5 hydrogenated petroleum resin, C9 hydrogenated petroleum resin and coumarone resin; the antioxidant is one or a mixture of antioxidant BHT, antioxidant DBH, antioxidant DNP, antioxidant RD, antioxidant MB, antioxidant MMB, antioxidant 2246, antioxidant 4010NA, antioxidant 4020 and antioxidant 1076; the solvent is one or a mixture of toluene, xylene, gasoline, n-hexane, cyclohexane, pentane and heptane.

6. A protective film for laser cutting of optical lenses as claimed in claim 5, characterized in that: The preparation method of the pressure-sensitive adhesive of the rubber-based pressure-sensitive adhesive layer is as follows: adjusting the temperature of the dissolving kettle to 50-60°C, stirring at a frequency of 30-50HZ, adding the solvent into the dissolving kettle, and then sequentially adding the tackifying resin, the antioxidant, and the base rubber into the kettle for stirring and dissolving, continuing to stir and dissolve for 10-12 hours, and then filtering the material to obtain the rubber-based pressure-sensitive adhesive.

7. The method for preparing a protective film for laser cutting of optical lenses according to claim 6, characterized in that: The steps include: S1, using a film blowing machine to co-extrude three layers to prepare a functional PE substrate layer; S2, respectively applying a release agent and a primer to the outer layer and the inner layer of the functional PE substrate layer by means of a screen roller coating, and drying to obtain a semi-finished product having a release layer, a functional PE substrate layer and a primer layer; S3, coating a layer of rubber-based pressure-sensitive adhesive on the surface of the primer coating layer by roller coating, and drying to obtain a protective film having a release layer, a functional PE substrate layer, a primer coating layer and a rubber-based pressure-sensitive adhesive layer.

8. The method for preparing a protective film for laser cutting of optical lenses according to claim 7, characterized in that: In step S1, the extrusion temperatures of the blown film are: 175-180°C for the outer layer, 140-175°C for the middle layer, and 175-180°C for the inner layer.

Citation Information

Patent Citations

  • Protective film with ultrahigh light transmittance and preparation method thereof

    CN112980346A

  • Pressure-sensitive adhesive film

    US20130344326A1

  • Pressure-sensitive adhesive film

    US20140113131A1