Water-soluble fluorescent material-resin composite and preparation method thereof, and tracer prepared therefrom
By reacting the water-soluble fluorescent material with monomer and initiator and grinding at low temperature, a water-soluble fluorescent material-resin composite with uniform particle size and high fluorescence intensity is solved, which is difficult to coat and easy to fall off in the prior art. Problem, the excellent optical performance of tracer and the possibility of large-scale production are achieved.
Patent Information
- Application Number
- CN202211316832.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-10-26
AI Technical Summary
The prior art is difficult to effectively coat water-soluble fluorescent materials, the preparation conditions are harsh, the cost is high, and the water-soluble fluorescent materials are prone to fall off, limiting the development of fluorescent microspheres and large-scale production.
A water-soluble fluorescent material is used to react with a mixture of monomers and initiators to form a cured product, and grind it at -80 to -30°C to form a water-soluble fluorescent material-resin composite with uniform particle size and high fluorescence intensity. By heat Curing and ball milling processes improve the coating effect.
The obtained water-soluble fluorescent material-resin composite has excellent optical properties, uniform particle size and high fluorescence intensity, and excellent optical properties suitable for tracers, which solves the problems of difficulty in covering and easy shedding, and realizes large-scale production. possibilities.
Smart Images

Figure CN115746825B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of display technology, and specifically relates to a water-soluble fluorescent material-resin composite and a preparation method thereof, and a tracer prepared therefrom. Background Art
[0002] Fluorescent microspheres refer to microspheres that use spherical particles ranging from tens of nanometers to hundreds of microns as carriers and are doped with luminescent materials such as water-soluble fluorescent materials to emit fluorescence. They are widely used in life sciences, clinical diagnosis, drug analysis, environmental monitoring and other fields.
[0003] Fluorescent microspheres prepared from organic polymers are widely used in cell labeling, high-throughput drug screening, and standard measurement due to their good monodispersity, stable optical properties, and rich surface functional groups. Common preparation methods for organic polymer fluorescent microspheres include emulsion polymerization, dispersion polymerization, and soap-free emulsion polymerization, and then the fluorescent microspheres are prepared by swelling, adsorption, copolymerization, and embedding. However, these methods can only be used to coat oil-soluble quantum dots, and it is difficult to coat water-soluble fluorescent materials. Even if they are coated, the coating content is very low. At the same time, the preparation conditions are harsh, the cost is high, and the water-soluble fluorescent materials are easy to fall off, making it difficult to mass produce. These have restricted the development of fluorescent microspheres. Summary of the invention
[0004] In view of the above technical problems, the present application provides a method for preparing a water-soluble fluorescent material-resin composite, comprising the following steps:
[0005] S1, mixing a water-soluble fluorescent material, a monomer and an initiator to react to form a solidified material;
[0006] S2. Grind the solidified material at -80 to -30°C to obtain a water-soluble fluorescent material-resin composite.
[0007] Further, the monomer is selected from at least one of styrene, methacrylic acid, methyl methacrylate, (chloromethyl)ethylene oxide, and epichlorohydrin;
[0008] Preferably, the water-soluble fluorescent material includes at least one of rhodamine B, lisserol rhodamine B, sodium fluorescein, Nile red, perylene red, tetramethylrhodamine isothiocyanate, 1,3,6,8-pyrenetetracarbonate tetrasodium salt, 9,10-diphenylanthracene, 9,10-bis(phenylethynyl)anthracene, 1-chloro-9,10-bis(phenylethynyl)anthracene, 1,8-dichloro-9,10-bis(phenylethynyl)anthracene, anthocyanin, and carbon quantum dots.
[0009] Furthermore, the mass ratio of the water-soluble fluorescent material to the monomer is 1:300 to 1:20000.
[0010] Furthermore, in the step S1, a thermal curing method is used to carry out the curing reaction.
[0011] Furthermore, in the step S2, the solidified material, the ball milling medium and the dispersant are added into a ball mill for grinding.
[0012] The present application also provides a water-soluble fluorescent material-resin composite, comprising a water-soluble fluorescent material and a coating coating the water-soluble fluorescent material, wherein the coating comprises a resin, and the resin is formed by curing a monomer.
[0013] Furthermore, the particle size of the water-soluble fluorescent material-resin composite is 1 μm-20 μm;
[0014] Preferably, the mass ratio of the water-soluble fluorescent material to the resin is 1:(700-40000).
[0015] Furthermore, the absolute value of the difference between the emission peaks of the water-soluble fluorescent material-resin composite and the water-soluble fluorescent material is 0 to 10 nm;
[0016] Preferably, the emission peak of the water-soluble fluorescent material-resin composite is 410-700 nm.
[0017] The present application also provides a tracer, comprising a support and the water-soluble fluorescent material-resin composite as described above.
[0018] Furthermore, the proppant material includes at least one of sand, ceramic particles, organic compound microspheres, and inorganic microspheres.
[0019] Furthermore, the proppant comprises pores, and the water-soluble fluorescent material-resin complex is located in the pores.
[0020] Beneficial effects: The preparation method of a water-soluble fluorescent material-resin composite of the present application comprises the following steps: S1, mixing a water-soluble fluorescent material, a monomer and an initiator to react to form a solidified product; S2, grinding the solidified product at -80 to -30°C to obtain a water-soluble fluorescent material-resin composite. The obtained water-soluble fluorescent material-resin composite has a uniform particle size and high fluorescence intensity, and has a small emission peak shift compared to the water-soluble fluorescent material, so that the obtained tracer has excellent optical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a fluorescence microscope image of the water-soluble fluorescent material-resin composite of Example 1 of the present application;
[0022] Figure 2 This is an emission spectrum diagram of the water-soluble fluorescent material-resin composite of Example 1 of the present application;
[0023] Figure 3 This is a fluorescence microscope image of the water-soluble fluorescent material-resin composite of Example 2 of the present application;
[0024] Figure 4 This is an emission spectrum diagram of the water-soluble fluorescent material-resin composite of Example 2 of the present application;
[0025] Figure 5 This is a fluorescence microscope image of the water-soluble fluorescent material-resin composite of Example 3 of the present application;
[0026] Figure 6 This is an emission spectrum diagram of the water-soluble fluorescent material-resin composite of Example 3 of the present application;
[0027] Figure 7 This is a fluorescence microscope image of the water-soluble fluorescent material-resin composite of Example 4 of the present application;
[0028] Figure 8 This is an emission spectrum diagram of the water-soluble fluorescent material-resin composite of Example 4 of the present application;
[0029] Fig. 9 This is an emission spectrum diagram of the water-soluble fluorescent material-resin composite of Comparative Example 1 of the present application;
[0030] Fig.10 This is a laser particle size diagram of the polystyrene fluorescent microspheres of Comparative Example 2 of the present application;
[0031] Fig.11 This is the emission spectrum of the polystyrene fluorescent microspheres of Comparative Example 2 of the present application. DETAILED DESCRIPTION
[0032] The following will describe the technical solutions in the embodiments of the present application in detail in combination with the embodiments of the present application. It should be noted that the described embodiments are only part of the embodiments of the present application, not all of the embodiments.
[0033] As described in the background technology, the preparation method of organic polymer fluorescent microspheres in the prior art is difficult to coat water-soluble fluorescent materials or the coating content is low. At the same time, the preparation conditions are harsh, the cost is high, the water-soluble fluorescent materials are easy to fall off, and it is difficult to produce on a large scale. These restrict the development of fluorescent microspheres.
[0034] Based on this, the present application provides a method for preparing a water-soluble fluorescent material-resin composite, comprising the following steps:
[0035] S1, mixing a water-soluble fluorescent material, a monomer and an initiator to react to form a solidified material;
[0036] The initiator of the present application initiates the polymerization of monomers to form a resin, and the resin encapsulates the water-soluble fluorescent material therein to form a relatively large-sized solidified product, the size of which is generally not less than 1 cm.
[0037] S2. Grind the solidified material at -80 to -30°C to obtain a water-soluble fluorescent material-resin composite.
[0038] At low temperatures of -80 to -30°C, the brittleness of the solidified material increases, and the solidified material is able to maintain a good morphology, which is conducive to subsequent ball milling treatment to obtain refined nanoparticles.
[0039] In a specific embodiment of the present application, the monomers in the preparation method of the water-soluble fluorescent material-resin composite are selected from at least one of styrene, methacrylic acid, methyl methacrylate, (chloromethyl)ethylene oxide, and epichlorohydrin. The resin formed by such monomers can effectively encapsulate the water-soluble fluorescent material, and the obtained water-soluble fluorescent material-resin composite has a uniform particle size.
[0040] The initiator of the present application can be a photoinitiator or a thermal initiator. The photoinitiator includes, for example, 2-hydroxy-2-methyl-1-phenylpropanone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-dimethylamino-2-benzyl-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, methyl benzoylformate, 2,4-dihydroxybenzophenone, diphenyl-(2,4,6-trimethylbenzoyl)phosphine, to produce excellent photoinitiation effect. The thermal initiator is, for example, selected from one or more of azo, peroxide, and persulfate.
[0041] In the present application, a cross-linking agent may be added to assist the polymerization of the monomers. The cross-linking agent includes, for example, conventional common cross-linking agents.
[0042] In a preferred embodiment, the water-soluble fluorescent material includes at least one of rhodamine B, lisian rhodamine B, sodium fluorescein, Nile red, perylene red, tetramethylrhodamine isothiocyanate, 1,3,6,8-pyrene tetracarbonate tetrasodium salt, 9,10-diphenylanthracene, 9,10-bis(phenylethynyl)anthracene, 1-chloro-9,10-bis(phenylethynyl)anthracene, 1,8-dichloro-9,10-bis(phenylethynyl)anthracene, anthocyanin, and carbon quantum dots. The obtained water-soluble fluorescent material-resin complex has a high fluorescence intensity. The water-soluble fluorescent material-resin complex of the present application preferably includes at least two water-soluble fluorescent materials, so that microspheres with more diverse encoding information can be obtained.
[0043] In a specific embodiment of the present application, in the preparation method of the water-soluble fluorescent material-resin composite, the mass ratio of the water-soluble fluorescent material to the monomer is 1:300 to 1:20000, so as to obtain a solidified product with uniform distribution of the water-soluble fluorescent material, which is conducive to the subsequent acquisition of a water-soluble fluorescent material-resin composite with uniform particle size and high fluorescence intensity.
[0044] In a specific embodiment of the present application, in the preparation method of the water-soluble fluorescent material-resin composite, thermal curing is used for curing in step S1, so as to facilitate large-scale curing, good cross-linking degree, and high hardness of the obtained cured product, which is conducive to subsequent grinding and refining. The water-soluble fluorescent material-resin composite of the present application is prepared.
[0045] In a preferred embodiment, the heating temperature in the heat curing method is 70 to 140° C., and the heat curing time is 2 to 6 hours, so as to obtain a better cross-linking degree, complete the curing reaction, and improve the hardness of the cured product.
[0046] In a specific embodiment of the present application, in the preparation method of the water-soluble fluorescent material-resin composite, in step S2, the solidified material, the ball milling medium and the dispersant are added to the ball mill for grinding, which has little effect on the optical properties of the water-soluble fluorescent material, so as to obtain a water-soluble fluorescent material-resin composite with a smaller particle size and higher fluorescence intensity.
[0047] In a preferred embodiment, the ball milling medium in the ball milling method is at least one of zirconium beads, glass beads, and steel beads, so as to better ball mill the solidified product.
[0048] In a preferred embodiment, the ball-to-material ratio of the ball-milling medium to the solidified material is 25:1 to 100:1, so as to obtain a water-soluble fluorescent material-resin composite with a more uniform particle size.
[0049] In a preferred embodiment, the ball milling time is 6 to 24 hours to obtain a water-soluble fluorescent material-resin composite with smaller and more uniform particle size.
[0050] In a preferred embodiment, the ball milling speed is 300-700 r / min to obtain a water-soluble fluorescent material-resin composite with more uniform particle size and higher content of water-soluble fluorescent material.
[0051] In a preferred embodiment, different sizes of ball milling media are used for high energy ball milling. For example, a ball milling medium with a diameter of Φ 1cm, Φ 0.7cm, Φ 0.5cm, Φ The ball milling medium of 0.3 cm can be adaptively configured with different mass ratios for ball milling the solidified material to obtain a water-soluble fluorescent material-resin composite with smaller and more uniform particle size and higher content of water-soluble fluorescent material.
[0052] In a preferred embodiment, the dispersant is at least one of ethanol, n-heptane and water to better assist in grinding the solidified material.
[0053] In a preferred embodiment, the mass ratio of the dispersant to the solidified material is 5:1 to 2:1, so as to obtain a water-soluble fluorescent material-resin composite with a more uniform particle size.
[0054] The present application also provides a water-soluble fluorescent material-resin composite, comprising a water-soluble fluorescent material and a coating encapsulating the water-soluble fluorescent material, wherein the coating comprises a resin, and the resin includes, for example, polystyrene, acrylic resin, and epoxy resin having a glass transition temperature lower than 60°C. The resin is formed by curing a monomer, and the resin has good coating properties for the water-soluble fluorescent material, thereby obtaining a water-soluble fluorescent material-resin composite with high fluorescence intensity and good stability.
[0055] In a specific embodiment of the present application, the particle size of the water-soluble fluorescent material-resin complex is 1 to 20 μm, so that the water-soluble fluorescent material-resin complex can be used as fluorescent coded microspheres in the field of tracing.
[0056] In a preferred embodiment, the mass ratio of the water-soluble fluorescent material to the resin in the water-soluble fluorescent material-resin composite is 1:40000 to 1:700, so as to obtain a water-soluble fluorescent material-resin composite with excellent optical properties.
[0057] In a specific embodiment of the present application, the absolute value of the difference between the emission peaks of the water-soluble fluorescent material-resin complex and the water-soluble fluorescent material is 0 to 10 nm, so that the emission peak of the prepared water-soluble fluorescent material-resin complex is slightly shifted compared to the emission peak of the water-soluble fluorescent material itself. When the water-soluble fluorescent material-resin complex is used as a fluorescent coded microsphere, the accuracy is higher.
[0058] In a preferred embodiment, the emission peak of the water-soluble fluorescent material-resin composite is 410-700 nm, so that a variety of fluorescent coded microspheres can be combined.
[0059] The present application also provides a tracer, including a proppant and the above-mentioned water-soluble fluorescent material-resin complex, wherein the proppant carries the water-soluble fluorescent material-resin complex and releases the water-soluble fluorescent material-resin complex slowly. The proppant and the water-soluble fluorescent material-resin complex are combined together and used as a composition, and the combination of the two includes physical force between the two, magnetic force, or coating the two in the same carrier, etc.
[0060] In a preferred embodiment of the present application, the proppant material includes at least one of sand, ceramic particles, organic compound microspheres, and inorganic microspheres. When the tracer is used in combination with hydraulic fracturing, there is a weak interaction force between the water-soluble fluorescent material-resin complex and the proppant. When the proppant is filled in the crack, the water-soluble fluorescent material-resin complex separates from the proppant at a slow rate, thereby prolonging the release time of the tracer.
[0061] Weak interaction forces, such as simple aggregation of water-soluble fluorescent material-resin complex and proppant through intermolecular forces, or using a proppant with a pore structure, encapsulating the water-soluble fluorescent material-resin complex in the pores of the proppant and then gradually releasing it, etc. The controlled slow release of the tracer may depend on the surface charge between the tracer and the proppant, which in turn may depend on the adsorption / desorption performance of the tracer on the adsorbent, pH changes, salinity, hydrocarbon composition, temperature and pressure, etc.
[0062] In a specific embodiment of the present application, the proppant includes a pore, and a water-soluble fluorescent material-resin complex is located in the pore. When used as an oilfield tracer, the tracer is added to the injection well using high-pressure water. With the injection of high-pressure water and the flow of the fluid, the water-soluble fluorescent material-resin complex combined with the proppant slowly detaches from the proppant, so that when sampling in the production well, the water-soluble fluorescent material-resin complex can be collected, thereby completing the collection of the tracer.
[0063] Some exemplary embodiments according to the present application are described in more detail below; however, the exemplary embodiments of the present application are not limited thereto.
[0064] Example 1
[0065] S1. Prepare a solidified material: add 1 mg of rhodamine B and 10 mg of sodium fluorescein to 1 ml of ethanol to prepare a water-soluble fluorescent material solution, add 0.8 g of azobisisobutyronitrile and 0.4 ml of divinylbenzene to the water-soluble fluorescent material solution, add the solution to 20 ml of styrene, ultrasonicate for 15 min, and heat at 70° C. for 2 h to obtain a solidified material;
[0066] S2. Preparation of water-soluble fluorescent material-resin composite: The solidified material was crushed at -30°C and ball-milled for 6 h at a speed of 500 r / min using a low-temperature ball mill. The ball-milling medium was 260 g of zirconium beads, the ball-to-material ratio was 30:1, and the size of the ball-milling medium was Φ 1cm, Φ 0.7cm, Φ 0.5cm, Φ 0.3cm, size is Φ 1cm, Φ 0.7cm, Φ0.5cm, Φ The mass ratio of the 0.3 cm ball milling medium is 2:1:1:1, the dispersant used is ethanol, and the mass ratio of the dispersant to the solidified material is 4:1. A water-soluble fluorescent material-resin composite with coded information is obtained. The fluorescence microscope image of the water-soluble fluorescent material-resin composite is as follows: Figure 1 As shown, it can be seen that the particle size of the water-soluble fluorescent material-resin composite is about 6 μm, and the particle size is uniform; the emission spectrum obtained is as follows Figure 2 As shown, the fluorescence emission peak is almost not shifted relative to the original emission peak of the corresponding fluorescent material (575 nm for rhodamine B and 525 nm for sodium fluorescein).
[0067] Example 2
[0068] This embodiment is substantially the same as embodiment 1, except that: the styrene in step S1 of embodiment 1 is replaced with epichlorohydrin, and a solidified product is obtained after heating at 80°C for 4 hours; the ball-to-material ratio in step S2 is set to 50:1, and the size of the ball milling medium is adjusted to Φ 1cm, Φ 0.5cm, Φ 0.3cm, size is Φ 1cm, Φ 0.5cm, Φ The mass ratio of the 0.3 cm ball milling medium is 2:2:1. The fluorescence microscope image of the water-soluble fluorescent material-resin composite is as follows: Figure 3 As shown, it can be seen that the particle size of the water-soluble fluorescent material-resin composite is about 2 μm, and the particle size is uniform; the obtained emission spectrum is as follows Figure 4 As shown, the fluorescence emission peak is slightly shifted relative to the original emission peak of the corresponding fluorescent material (575 nm for rhodamine B and 525 nm for sodium fluorescein).
[0069] Example 3
[0070] This embodiment is substantially the same as embodiment 2, except that the rhodamine B in embodiment 2 is replaced with perylene red, and the fluorescence microscope image of the obtained water-soluble fluorescent material-resin complex is as follows: Figure 5 As shown, it can be seen that the particle size of the water-soluble fluorescent material-resin composite is about 10 μm, and the particle size is relatively uniform; the obtained emission spectrum is as follows Figure 6 As shown, the fluorescence emission peak is slightly shifted relative to the original emission peak of the corresponding fluorescent material (612 nm for perylene red and 525 nm for sodium fluorescein).
[0071] Example 4
[0072] This embodiment is substantially the same as embodiment 2, except that the rhodamine B and sodium fluorescein in step S1 of embodiment 2 are replaced with 10 mg of green carbon dots, and the fluorescence microscope image of the obtained water-soluble fluorescent material-resin complex is as follows: Figure 7 As shown, it can be seen that the particle size of the water-soluble fluorescent material-resin composite is about 5 μm, and the particle size is relatively uniform; the obtained emission spectrum is as follows Figure 8 As shown, the fluorescence emission peak is slightly shifted relative to the original emission peak (525 nm) of the green carbon dots.
[0073] Comparative Example 1
[0074] This embodiment is substantially the same as the embodiment 1, except that the ball milling temperature in the embodiment 1 is adjusted to 25° C., the fluorescence signal of the water-soluble fluorescent material-resin composite basically disappears, and the emission spectrum of the water-soluble fluorescent material-resin composite is compared. Fig. 9 As shown, the fluorescence emission peak is greatly shifted relative to the original emission peak of the corresponding fluorescent material (575 nm for rhodamine B and 525 nm for sodium fluorescein).
[0075] Comparative Example 2
[0076] Preparation of solidified material: 10 mg of rhodamine B and 10 mg of sodium fluorescein were added to 30 ml of deionized water to prepare a water-soluble fluorescent material solution. 6.6 ml of styrene and 0.9 g of PVP were added to the water-soluble fluorescent material solution. Nitrogen was bubbled for 30 min, the temperature was raised to 70 degrees, 0.15 g of azobisisobutyronitrile was added, and the temperature was kept at 70 degrees overnight to obtain polystyrene fluorescent microspheres. The laser particle size analyzer particle size of the obtained polystyrene fluorescent microspheres was as follows: Fig.10 As shown in Figure 1, it can be seen that the particle size of the polystyrene fluorescent microspheres is about 765nm, and the particle size is relatively uniform; the emission spectrum obtained is as follows: Fig.11 As shown, the fluorescence emission peak is greatly shifted relative to the original emission peak of the corresponding fluorescent material (575 nm for rhodamine B and 525 nm for sodium fluorescein).
[0077] The particle sizes of the water-soluble fluorescent material-resin composites of Examples 1 to 4 and Comparative Examples 1 to 2 were tested using a Malvern laser particle size analyzer and an Olympus-IX71 fluorescence microscope, and the emission wavelengths were tested using fluorescence spectrometers F-4500 and QE-65000.
[0078] Compared with comparative examples 1 to 2, the water-soluble fluorescent material-resin composites of Examples 1 to 4 of the present application have uniform particle size, high fluorescence intensity, and almost no displacement of the fluorescence emission peak. The water-soluble fluorescent material-resin composites have good stability when used as tracers.
[0079] Although the inventors have elaborated and enumerated the technical solutions of the present application in detail, it should be understood that it is obvious for those skilled in the art to modify and / or adapt the above embodiments or adopt equivalent alternative solutions, which cannot deviate from the essence of the spirit of the present application. The terms appearing in the present application are used to explain and understand the technical solutions of the present application and cannot constitute limitations on the present application.
Claims
1. A method for preparing a water-soluble fluorescent material-resin composite, It is characterized in that The steps include: S1. Mix a water-soluble fluorescent material, a monomer and an initiator to react to form a solidified product; the size of the solidified product is ≥1 cm; the water-soluble fluorescent material includes at least one of rhodamine B, lissamine rhodamine B, sodium fluorescein, perylene red, tetramethyl rhodamine isothiocyanate, 1,3,6,8-pyrene tetracarbonate tetrasodium salt, and anthocyanin; the monomer is selected from at least one of styrene, methacrylic acid, methyl methacrylate, (chloromethyl) ethylene oxide, and epichlorohydrin; the initiator includes a photoinitiator or a thermal initiator; S2. Grinding the solidified material at -80 to -30°C to obtain a water-soluble fluorescent material-resin composite; the particle size of the water-soluble fluorescent material-resin composite is 1 μm to 20 μm.
2. The method for preparing the water-soluble fluorescent material-resin composite according to claim 1, It is characterized in that The mass ratio of the water-soluble fluorescent material to the monomer is 1:300-1:20000.
3. The method for preparing the water-soluble fluorescent material-resin composite according to claim 1, It is characterized in that In the step S2, the solidified material, the ball milling medium and the dispersant are added into a ball mill for grinding.
4. The method for preparing the water-soluble fluorescent material-resin composite according to claim 1, It is characterized in that The absolute value of the difference between the emission peaks of the water-soluble fluorescent material-resin composite and the water-soluble fluorescent material is 0-10 nm.
5. A tracer, It is characterized in that The invention comprises a supporting agent and a water-soluble fluorescent material-resin composite prepared by the method for preparing a water-soluble fluorescent material-resin composite according to any one of claims 1 to 4.
6. The tracer according to claim 5, It is characterized in that The proppant material includes at least one of sand, ceramic particles, organic compound microspheres, and inorganic microspheres.
7. The tracer according to claim 5, It is characterized in that The proppant comprises pores, and the water-soluble fluorescent material-resin complex is located in the pores.
Citation Information
Patent Citations
Oilfield tracer, oilfield tracing method and proppant composition
CN111100612A
Resin particles for fluorescent labels
US20160011179A1