A cutting tool and its cutting edge laser cladding strengthening method
By using laser cladding to form a wear-resistant layer in the cutting edge of the low carbon alloy steel tool in the tool, the problems of low tool hardness and poor wear resistance are solved, the wear resistance and service life of the tool are significantly improved, and the manufacturing cost is reduced. .
Patent Information
- Application Number
- CN202211472584.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-11-23
AI Technical Summary
The existing tools have low hardness and poor wear resistance, making it difficult to repeat grinding and maintain sharpness, which affects service life.
The tool body is made of medium-carbon low-alloy steel, and a wear-resistant layer with a width of 1.3-2.8 mm and a height of 3-10 mm is formed at the cutting edge by laser cladding. The alloy powder contains high contents of Cr, B, Ni, Ce, and Elements such as Y form an wear-resistant layer with high hardness and good wear resistance through laser cladding.
It significantly improves the tensile strength, impact toughness and wear resistance of the tool, extends the tool life, and increases the service life by more than 350% and 300% compared with high-speed steel and stainless steel tools, reducing manufacturing costs.
Smart Images

Figure 980679DEST_PATH_IMAGE001
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cutting tools, and in particular to a cutting tool and a cutting edge laser cladding strengthening method thereof. Background Art
[0002] In my country, the technical development of kitchen hardware knives has gone through two different stages of development. The first stage was mainly carbon steel knives, with the cutting edge materials being 45#, 55#, and 65Mn. The second stage was mainly stainless steel knives, with 20Cr13 and 30Cr13 as the starting materials. In order to improve wear resistance, the material selection was adopted to increase the carbon chromium content and add Mo and V alloys, thus developing into 40Cr13, 50Cr13, 60Cr13, 70Cr13, 80Cr18, 90Cr18, and 50Cr15MoV, 60Cr13Mo, 90Cr18Mo with Mo added. However, although adding Mo and V elements can improve the wear resistance of knives, the prices of Mo and V elements are high. Adding more Mo and V elements to the tool material causes a huge waste of resources and leads to a sharp increase in the manufacturing cost of the tool.
[0003] In order to improve the wear resistance of knives, Chinese invention patent CN103045963 discloses a low-chromium, high-silicon, vanadium, nitrogen and boron multi-component reinforced wear-resistant kitchen knife steel strip, characterized in that: the specific components it contains, calculated by weight percentage, are: C: 0.50-0.60%; Mn: 0.3-0.7%; Si: 2.5-3.5%; P≤0.010%; S≤0.010%; Cr: 9.00-10.00%; Ni≤0.6%; V: 0.16-0.32%; N: 0.04-0.08%; B: 0.0008-0.002%; the balance is Fe. The low-chromium, high-silicon, vanadium, nitrogen and boron multi-component reinforced wear-resistant kitchen knife steel strip has high matrix strength, good knife edge sharpness, wear resistance and corrosion resistance, and low production cost. It is mainly used for kitchen knives and can also be used in the production of scissors.
[0004] Chinese utility model CN208946220 provides a high-hardness, corrosion-resistant ceramic steel kitchen knife, including a stainless steel knife blank and a handle, the rear of the stainless steel knife blank is provided with a rectangular connector, the connector can be inserted into the handle; the lower part of the stainless steel knife blank is provided with a blade, the blade is provided with a plurality of knife holes arranged at intervals, the surface of the blade is covered with a metal ceramic powder metallurgy fusion layer or a cemented carbide mixed powder layer, which is strengthened on the blade of the knife by laser cladding or argon arc welding, and 1-N small holes are opened at the blade of the knife blank to form a firm metallurgical bond between the metal ceramic powder and the stainless steel knife blank, and its hardness reaches 62-70 degrees Rockwell. The knife hole is filled with a metal ceramic powder metallurgy fusion layer. The kitchen knife is corrosion-resistant, and the knife blank is sharpened, and the hardness, sharpness and wear resistance of the knife part are greatly improved, and the sharpness of the blade can be maintained for a long time, and the knife body has the advantages of high hardness and good toughness at the blade.
[0005] Chinese invention patent CN106676247 also discloses a method for treating kitchen knives, and particularly relates to a method for treating kitchen knives with vacuum oil quenching. The invention provides the following technical solution: a method for treating kitchen knives with vacuum oil quenching, comprising the steps of: a. placing the processed kitchen knives in batches in a vacuum oil quenching furnace; b. heating and heat preservation of the kitchen knives in the vacuum oil quenching furnace in five stages; c. oil quenching the kitchen knives after step b. The above technical solution provides a method for treating kitchen knives with vacuum oil quenching that can improve the oxidation resistance, uniform hardness, and resistance to breakage of kitchen knives.
[0006] However, the above-mentioned methods for manufacturing cutting tools still have the problems of low cutting hardness and poor wear resistance. In most cases, the regrindability of cutting tools is not considered, which makes it difficult to repeatedly grind the cutting tools to keep the cutting edge sharp after use, thus shortening the service life of the cutting tools. With the requirements of social development, it will become inevitable to develop cutting tools with good regrindability, high cutting sharpness and good economic efficiency. Summary of the invention
[0007] In view of the above problems, the present invention aims to solve the above problems. One object of the present invention is to provide a cutting tool and a cutting edge laser cladding strengthening method thereof to solve the above problems.
[0008] The purpose of the present invention is to form a wear-resistant layer with a width of 1.3-2.8mm and a height of 3-10mm on the working part of the blade of a medium-carbon low-alloy steel tool by laser cladding, thereby significantly extending the tool life. The specific preparation process steps are:
[0009] First, the medium carbon low alloy steel of the tool body material is melted in an electric furnace. The chemical composition and mass fraction of the medium carbon low alloy steel are: 0.42-0.49% C, 0.21-0.29% Si, 3.36-3.48% Mn, 0.17-0.33% Cr, 0.013-0.019% B, 0.020-0.027% Ca, 0.06-0.09% Ti, 0.013-0.019% Mg, 0.11-0.16% Nb, 0.027-0.039% N, 0.00-0.025% S, 0.00-0.028% P, and the balance is Fe and unavoidable impurities; the medium carbon low alloy steel is first cast into a blank, and then heat treated;
[0010] The specific heat treatment includes: heating the blank to 1120-1150℃, keeping it warm for 2-3 hours, and then forging it into a tool body with a forging ratio of 4-6; reheating the forged tool body to 890-920℃, keeping it warm for 1-1.5 hours, and then cooling it to room temperature after being taken out of the furnace, and then reheating it to 320-340℃, keeping it warm for 4-5 hours, and then cooling it to a temperature below 150℃ in the furnace, and then cooling it to room temperature after being taken out of the furnace, and then rough processing;
[0011] The blade of the rough-machined tool body is first preheated with a fiber laser for 15-25 seconds, with a preheating power of 300-500W; then a powder feeding system consisting of a powder feeder, a coaxial powder feeding head, and a powder feeding and control system is used to laser-clad the blade of the tool body with an alloy powder having a mass fraction of 28.03-29.16% Cr, 0.22-0.28% C, 3.27-3.40% Si, 2.91-3.15% B, 5.04-5.22% Ni, 0.32-0.55% Mn, 0.23-0.31% Ce, 10.06-10.34% W, 0.57-0.64% Y, 0.00-0.030% S, 0.00-0.035% P, and the remainder being Fe and unavoidable impurities, and the alloy powder size is 65-80μm;
[0012] Laser cladding uses a fiber laser. The process parameters of laser cladding are: laser power: 3500-4000W, scanning speed: 8-10mm / s, powder feeding rate: 20-25g / min, spot size: 5mm×5mm, argon flow rate: 18-20L / min; the cladding forms a wear-resistant layer with a width of 1.3-2.8mm and a height of 3-10mm, and finally it is finished to the specified size and accuracy.
[0013] A tool comprises a tool body and a wear-resistant layer, wherein the wear-resistant layer is arranged on the blade of the tool body.
[0014] In order to save the cost of the tool, the present invention adopts medium carbon low alloy steel to produce the tool body. The tool body is smelted in an electric furnace, with simple process and high production efficiency. The chemical composition and mass fraction of the medium carbon low alloy steel of the tool body material are: 0.42-0.49% C, 0.21-0.29% Si, 3.36-3.48% Mn, 0.17-0.33% Cr, 0.013-0.019% B, 0.020-0.027% Ca, 0.06-0.09% Ti, 0.013-0.019% Mg, 0.11-0.16% Nb, 0.027-0.039% N, 0.00-0.025% S, 0.00-0.028% P, and the balance is Fe and unavoidable impurities. The addition of 3.36-3.48% Mn and 0.013-0.019% B ensures that the material obtains a strong and tough bainite structure after air cooling and quenching. The addition of 0.21-0.29% Si and 0.17-0.33% Cr is beneficial to improve the strength of the steel. In particular, the addition of 0.020-0.027% Ca, 0.06-0.09% Ti, 0.013-0.019% Mg, 0.11-0.16% Nb, and 0.027-0.039% N is beneficial to grain refinement, improving the morphology and distribution of inclusions, and improving the comprehensive performance of the tool body. In order to further improve the toughness of the tool body and prevent deformation and breakage during the use of the tool, after the medium-carbon low-alloy steel is poured into a blank, the blank is heated to 1120-1150℃, kept warm for 2-3 hours, and forged into the tool body with a forging ratio of 4-6, which can improve the tool density, refine the grains, and further improve the toughness of the tool. The forged tool body is reheated to 890-920℃, kept warm for 1-1.5 hours, and then air-cooled to room temperature to obtain a uniform bainite structure. Then it is reheated to 320-340℃, kept warm for 4-5 hours, and then cooled to a temperature below 150℃ in the furnace, and then air-cooled to room temperature in the furnace to eliminate tool stress and stabilize the structure.
[0015] The present invention preheats the blade of the tool body after rough machining by using a fiber laser for 15-25 seconds with a preheating power of 300-500W to increase the temperature of the blade of the tool body and prevent cracks from appearing in the laser cladding wear-resistant alloy layer. After the cutting edge is preheated by laser, a powder feeding system consisting of a powder feeder, a coaxial powder feeding head, and a powder feeding and control system is used to laser clad the cutting edge of the tool body with alloy powders having a mass fraction of 28.03-29.16% Cr, 0.22-0.28% C, 3.27-3.40% Si, 2.91-3.15% B, 5.04-5.22% Ni, 0.32-0.55% Mn, 0.23-0.31% Ce, 10.06-10.34% W, 0.57-0.64% Y, 0.00-0.030% S, 0.00-0.035% P, and the remainder being Fe and unavoidable impurities. The alloy powder size is 65-80μm. The powder feeding system is used to deliver powder to achieve laser cladding, which is efficient and easy to control the width and height of the cladding layer. The alloy powder contains 28.03-29.16% Cr, which can ensure that the edge of the laser cladding wear-resistant layer after laser cladding has good corrosion resistance. In addition, chromium and boron are combined to form Cr2B, which has high hardness and improves the hardness and wear resistance of the laser cladding wear-resistant layer. Adding 2.91-3.15% B, in addition to generating high-hardness Cr2B, part of B is dissolved in the matrix to provide matrix hardness and wear resistance. Adding 5.04-5.22% Ni, 0.23-0.31% Ce, and 0.57-0.64% Y can improve the strength and toughness of the laser cladding wear-resistant layer and prevent the edge from cracking during use. Adding 10.06-10.34% W, in addition to improving the room temperature hardness of the wear-resistant layer, part of W is dissolved in the matrix, improving the high-temperature stability of the laser cladding wear-resistant layer and promoting further improvement of wear resistance. The laser cladding of the present invention uses a fiber laser, and the obtained coating has good surface quality without defects such as cracks and pores. The preferred laser cladding process parameters of the present invention are: laser power: 3500-4000W, scanning speed: 8-10mm / s, powder feeding rate: 20-25g / min, spot size: 5mm×5mm, argon gas flow rate: 18-20L / min; laser cladding forms a wear-resistant layer with a width of 1.3-2.8mm and a height of 3-10mm. The tool after laser cladding of the blade is finally finished to the specified size and accuracy to obtain a tool product with excellent wear resistance.
[0016] Compared with the prior art, the present invention has the following advantages:
[0017] 1) The tensile strength of the tool body of the present invention is greater than 2150MPa, and the impact toughness is α kU More than 80J / cm 2, with excellent toughness, the tool body uses cheap Mn as the main alloy element, does not contain expensive alloy elements such as molybdenum, vanadium, and nickel, and the manufacturing cost of the tool body is more than 60% lower than that of high-speed steel tools and stainless steel tools;
[0018] 2) After laser surface strengthening treatment, the cutting edge of the tool of the present invention has a hardness of more than 1220HV, has excellent wear resistance and corrosion resistance, and can be repeatedly ground after use to keep the cutting edge sharp, which greatly improves the service life of the tool. The service life of the tool is increased by 350% and 300% respectively compared with that of high-speed steel tools and stainless steel tools. The promotion and application of the tool has good economic and social benefits. DETAILED DESCRIPTION
[0019] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. It should be noted that the embodiments and features in the embodiments of this application can be combined with each other arbitrarily without conflict.
[0020] The blade laser cladding strengthening method and the tool are described in detail.
[0021] A cutting tool and a cutting edge laser cladding strengthening method thereof, comprising:
[0022] Step S1: using medium carbon low alloy steel to manufacture the tool body;
[0023] Step S2: using a laser cladding method to form a wear-resistant layer with a width of 1.3-2.8 mm and a height of 3-10 mm on the blade of the tool body;
[0024] Among them, the laser cladding method specifically includes:
[0025] Preheat the fiber laser for 15-25 seconds at a preheating power of 300-500W;
[0026] The alloy powder components are then laser clad onto the cutting edge of the tool body;
[0027] The alloy powder composition includes 28.03-29.16% Cr, 0.22-0.28% C, 3.27-3.40% Si, 2.91-3.15% B, 5.04-5.22% Ni, 0.32-0.55% Mn, 0.23-0.31% Ce, 10.06-10.34% W, 0.57-0.64% Y, 0.00-0.030% S, 0.00-0.035% P, and the balance is Fe.
[0028] The particle size of the alloy powder is 65-80 μm.
[0029] Step S1 uses medium carbon low alloy steel to manufacture the tool body, including: smelting carbon low alloy steel in an electric furnace, casting the low alloy steel into a tool blank after smelting, and then performing heat treatment; wherein the chemical composition of the medium carbon low alloy steel includes: 0.42-0.49% C, 0.21-0.29% Si, 3.36-3.48% Mn, 0.17-0.33% Cr, 0.013-0.019% B, 0.020-0.027% Ca, 0.06-0.09% Ti, 0.013-0.019% Mg, 0.11-0.16% Nb, 0.027-0.039% N, 0.00-0.025% S, 0.00-0.028% P, and the remainder is Fe.
[0030] Step S1 heat treatment includes: heating the tool blank to 1120-1150°C, keeping it warm for 2-3 hours, and forging it into a tool body with a forging ratio of 4-6; reheating the forged tool body to 890-920°C, keeping it warm for 1-1.5 hours, taking it out of the furnace and air cooling it to room temperature, and then reheating it to 320-340°C, keeping it warm for 4-5 hours, cooling it in the furnace to a temperature below 150°C, taking it out of the furnace and air cooling it to room temperature, and then performing rough processing to prepare for laser cladding of the tool blade.
[0031] The laser cladding process parameters of the laser cladding method in step S2 include: laser power: 3500-4000 W, scanning speed: 8-10 mm / s, powder feeding rate: 20-25 g / min, spot size: 5 mm×5 mm, and argon gas flow rate: 18-20 L / min.
[0032] A tool prepared by a tool blade laser cladding strengthening method comprises a tool body and a wear-resistant layer, wherein the wear-resistant layer is arranged on the blade portion of the tool body.
[0033] A cutting tool and a cutting edge laser cladding strengthening method thereof, characterized in that the cutting tool body is made of medium carbon low alloy steel, and a wear-resistant layer with a width of 1.3-1.4 mm and a height of 3.0-3.2 mm is clad by laser on the cutting edge of the cutting tool body. The specific preparation process steps are as follows:
[0034] First, the medium carbon low alloy steel of the tool body material is melted in an electric furnace. The chemical composition and mass fraction of the medium carbon low alloy steel are: 0.42% C, 0.29% Si, 3.36% Mn, 0.33% Cr, 0.013% B, 0.027% Ca, 0.06% Ti, 0.019% Mg, 0.11% Nb, 0.039% N, 0.021% S, 0.026% P, and the balance is Fe and unavoidable impurities; the medium carbon low alloy steel is first cast into a blank, and then the blank is heated to 1120 ° C, kept warm for 3 hours, and then forged into a tool body, with a forging ratio of 4;
[0035] The forged tool body is reheated to 920°C, kept at this temperature for 1 hour, taken out of the furnace and air-cooled to room temperature, then reheated to 320°C, kept at this temperature for 5 hours, cooled in the furnace to a temperature below 150°C, taken out of the furnace and air-cooled to room temperature, and then rough-machined;
[0036] The blade of the tool body after rough machining was first preheated with a fiber laser for 25 seconds with a preheating power of 300W; then a powder feeding system consisting of a powder feeder, a coaxial powder feeding head and a powder feeding and control system was used to feed 28.03% Cr, 0.28% C, 3.27% Si, 3.15% B, 5.04% Ni, 0.55% Mn, 0.23% Ce, 10.06% W, 0.64% Y, 0.025% S, 0.031% P, and the remainder Fe and The alloy powder with inevitable impurities is laser clad to the blade of the tool body, and the alloy powder size is 65-80μm; the laser cladding uses a fiber laser, and the laser cladding process parameters are: laser power: 3500W, scanning speed: 8mm / s, powder feeding rate: 20g / min, spot size: 5mm×5mm, argon flow rate: 18L / min; the laser cladding wear-resistant layer has a width of 1.3-1.4mm and a height of 3.0-3.2mm, and is finally finished to the specified size and accuracy. The mechanical properties of the tool are shown in Table 1.
[0037] Table 1 Mechanical properties of tool
[0038]
[0039] Embodiment 2:
[0040] A cutting tool and a cutting edge laser cladding strengthening method thereof, characterized in that the cutting tool body is made of medium carbon low alloy steel, and a wear-resistant layer with a width of 2.7-2.8 mm and a height of 9.9-10 mm is clad by laser on the cutting edge of the cutting tool body. The specific preparation process steps are as follows:
[0041] First, the medium carbon low alloy steel of the tool body material is melted in an electric furnace. The chemical composition and mass fraction of the medium carbon low alloy steel are: 0.49% C, 0.21% Si, 3.48% Mn, 0.17% Cr, 0.019% B, 0.020% Ca, 0.09% Ti, 0.013% Mg, 0.16% Nb, 0.027% N, 0.011% S, 0.020% P, and the balance is Fe and unavoidable impurities; the medium carbon low alloy steel is first cast into a blank, and then the blank is heated to 1150 ° C, kept warm for 2 hours, and then forged into a tool body, with a forging ratio of 6;
[0042] The forged tool body is reheated to 910°C, kept at this temperature for 1 hour, taken out of the furnace and air-cooled to room temperature, then reheated to 330°C, kept at this temperature for 4.5 hours, cooled in the furnace to a temperature below 150°C, taken out of the furnace and air-cooled to room temperature, and then rough-machined;
[0043] The blade of the rough-machined tool body is first preheated with a fiber laser for 20 seconds with a preheating power of 400W; then a powder feeding system consisting of a powder feeder, a coaxial powder feeding head, and a powder feeding and control system is used to feed 29.16% Cr, 0.22% C, 3.40% Si, 2.91% B, 5.22% Ni, 0.32% Mn, 0.31% Ce, 10.06% W, 0.57% Y, 0.021% S, 0.034% P, and the remainder Fe and The alloy powder with inevitable impurities is laser clad to the blade of the tool body, and the alloy powder size is 65-80μm; the laser cladding uses a fiber laser, and the process parameters of the laser cladding are: laser power: 4000W, scanning speed: 10mm / s, powder feeding rate: 25g / min, spot size: 5mm×5mm, argon flow rate: 20L / min; the laser cladding wear-resistant layer has a width of 2.7-2.8mm and a height of 9.9-10mm, and is finally finished to the specified size and accuracy. The mechanical properties of the tool are shown in Table 1.
[0044] Embodiment 3:
[0045] A cutting tool and a cutting edge laser cladding strengthening method thereof, characterized in that the cutting tool body is made of medium carbon low alloy steel, and a wear-resistant layer with a width of 1.9-2.0 mm and a height of 6.1-6.2 mm is clad by laser on the cutting edge of the cutting tool body. The specific preparation process steps are as follows:
[0046] First, the medium carbon low alloy steel of the tool body material is melted in an electric furnace. The chemical composition and mass fraction of the medium carbon low alloy steel are: 0.46% C, 0.25% Si, 3.39% Mn, 0.26% Cr, 0.018% B, 0.022% Ca, 0.08% Ti, 0.015% Mg, 0.14% Nb, 0.029% N, 0.020% S, 0.027% P, and the balance is Fe and unavoidable impurities; the medium carbon low alloy steel is first cast into a blank, and then the blank is heated to 1140 ° C, kept warm for 3 hours, and then forged into a tool body, with a forging ratio of 5;
[0047] The forged tool body is reheated to 890°C, kept at this temperature for 1.5 hours, taken out of the furnace and air-cooled to room temperature, then reheated to 340°C, kept at this temperature for 4 hours, cooled in the furnace to a temperature below 150°C, taken out of the furnace and air-cooled to room temperature, and then rough-machined;
[0048] The blade of the tool body after rough machining was first preheated with a fiber laser for 15 seconds with a preheating power of 500W; then a powder feeding system consisting of a powder feeder, a coaxial powder feeding head and a powder feeding and control system was used to feed 28.60% Cr, 0.25% C, 3.27-3.40% Si, 2.99% B, 5.17% Ni, 0.38% Mn, 0.27% Ce, 10.13% W, 0.59% Y, 0.027% S, 0.033% P, and the remainder F e and inevitable impurities of alloy powder, laser cladding to the blade of the tool body, alloy powder size 65-80μm; laser cladding uses fiber laser, laser cladding process parameters, laser power: 3800W, scanning speed: 9mm / s, powder feeding rate: 22g / min, spot size: 5mm×5mm, argon flow: 19L / min; laser cladding wear-resistant layer width 1.9-2.0mm, height 6.1-6.2mm, finally fine machining to the specified size and accuracy. Tool mechanical properties are shown in Table 1.
[0049] The tool body of the present invention has a tensile strength greater than 2150MPa, an impact toughness αkU greater than 80J / cm2, and has excellent toughness. The tool body uses cheap Mn as the main alloying element, and does not contain expensive alloying elements such as molybdenum, vanadium, and nickel. The manufacturing cost of the tool body is reduced by more than 60% compared with high-speed steel tools and stainless steel tools. After laser surface strengthening treatment, the cutting edge of the tool of the present invention has a hardness of more than 1220HV, has excellent wear resistance and corrosion resistance, and the tool can be repeatedly ground after use to keep the blade sharp, which greatly improves the service life of the tool. The tool service life is increased by 350% and 300% respectively compared with high-speed steel tools and stainless steel tools. The promotion and application of the tool of the present invention has good economic and social benefits.
[0050] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. The terms "include", "comprises" or any other variants thereof are intended to cover non-exclusive inclusion, so that an article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such article or device. In the absence of further restrictions, the elements defined by the sentence "includes..." do not exclude the existence of other identical elements in the article or device including the elements.
[0051] The above embodiments are only used to illustrate the technical solution of the present invention and are not intended to limit the present invention. The present invention is described in detail with reference to the preferred embodiments. It should be understood by those skilled in the art that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, and should be included in the scope of the claims of the present invention.
Claims
1. A method for laser cladding strengthening of a tool blade, characterized in that: include: Step S1: using medium carbon low alloy steel to manufacture the tool body; Step S2: using a laser cladding method to form a wear-resistant layer with a width of 1.3-2.8 mm and a height of 3-10 mm on the blade of the tool body; Among them, the laser cladding method specifically includes: Preheat the fiber laser for 15-25 seconds at a preheating power of 300-500W; The alloy powder components are then laser clad onto the cutting edge of the tool body; The alloy powder composition includes 28.03-29.16% Cr, 0.22-0.28% C, 3.27-3.40% Si, 2.91-3.15% B, 5.04-5.22% Ni, 0.32-0.55% Mn, 0.23-0.31% Ce, 10.06-10.34% W, 0.57-0.64% Y, 0.00-0.030% S, 0.00-0.035% P, and the balance is Fe; Among them, the alloy powder particle size is 65-80μm; Step S1 uses medium carbon low alloy steel to manufacture the tool body, including: The carbon low alloy steel is melted in an electric furnace, and the low alloy steel is poured into a tool blank after melting, and then heat treated; Among them, the chemical composition of medium carbon low alloy steel includes: 0.42-0.49% C, 0.21-0.29% Si, 3.36-3.48% Mn, 0.17-0.33% Cr, 0.013-0.019% B, 0.020-0.027% Ca, 0.06-0.09% Ti, 0.013-0.019% Mg, 0.11-0.16% Nb, 0.027-0.039% N, 0.00-0.025% S, 0.00-0.028% P, and the balance is Fe; The heat treatment in step S1 includes: Heat the tool blank to 1120-1150℃, keep it warm for 2-3 hours, and then forge it into the tool body with a forging ratio of 4-6; The forged tool body is reheated to 890-920℃, kept at this temperature for 1-1.5 hours, taken out of the furnace and air-cooled to room temperature, then reheated to 320-340℃, kept at this temperature for 4-5 hours, furnace-cooled to a temperature below 150℃, taken out of the furnace and air-cooled to room temperature, and then rough-processed in preparation for laser cladding of the tool blade.
2. The method for strengthening a tool blade by laser cladding according to claim 1, characterized in that: The laser cladding process parameters of the laser cladding method in step S2 include: Laser power: 3500-4000W, scanning speed: 8-10mm / s, powder feeding rate: 20-25g / min, spot size: 5mm×5mm, argon flow rate: 18-20L / min.
3. A tool prepared by the tool edge laser cladding strengthening method according to any one of claims 1-2, characterized in that: include: A tool body and a wear-resistant layer, wherein the wear-resistant layer is arranged on the blade portion of the tool body.