Aerogel-based energy-absorbing material, preparation method and application thereof
By loading energy-absorbing substances and functional additives in porous aerogel materials, a nanofiber-based material connecting three-dimensional porous network structure is solved, and the lack of shear thickening materials in application is achieved, and high-efficiency energy-absorbing performance and light quality are achieved. Comfortable protective effect.
Patent Information
- Application Number
- CN202211521126.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-11-30
AI Technical Summary
In actual applications, existing shear thickening materials have problems such as uneven particle dispersion, narrow rheology performance, easy water absorption, temperature sensitivity and interface failure, which cannot meet the needs of lightweight, comfortable and protective performance.
Develop an aerogel-based energy-absorbing material, using porous aerogel materials as the substrate, loaded energy-absorbing substances and functional additives, and prepared by in-situ polymerization or solution-assisted filling technology to form a nanofiber base with a three-dimensional porous network structure connected to it Materials can absorb impact energy when strain or shear rate changes.
Overcoming the shortcomings of traditional materials, it provides designable morphological structure, high strength and sensitivity energy absorption performance, suitable for shock absorption, impact protection and energy absorption fields, and is easy to produce on a large scale.
Smart Images

Figure CN115748238B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an energy absorbing material, in particular to an aerogel-based energy absorbing material, a preparation method and application thereof, and belongs to the technical field of new nano materials. Background Art
[0002] In recent years, as people's awareness of personal protection, protection during the transportation or use of instruments and equipment continues to increase, the demand for lightweight protective energy-absorbing materials has gradually increased. For example, in high-risk working environments, personal protection needs to be done to ensure personal safety; in industrial production such as bridges and buildings, dampers are needed to dissipate unnecessary or harmful energy to the system; in the fields of automobiles, aerospace, etc., a large amount of impact energy needs to be absorbed to ensure the safety and normal operation of personnel, vehicles and spacecraft. Therefore, protective equipment with excellent energy absorption performance and light weight and comfort is in urgent need of development.
[0003] Shear thickening materials, as a typical representative of materials with good energy absorption properties, have a very wide range of application scenarios. Shear thickening materials are also called non-Newtonian fluids, which usually exhibit special fluid behaviors. Their most distinctive characteristic is the shear thickening effect, that is, under a certain range of shear rates, the viscosity of the shear thickening material will increase sharply with the increase of the shear rate. When it is not subjected to force, it is light and soft. At this time, it is comfortable to wear and easy to deform. When impacted by external forces, the material will quickly harden, showing good absorption of impact energy. After the impact, the material will return to its soft state. In recent years, shear thickening materials have attracted the attention of academia and industry in the fields of human protection due to their excellent lightness, protection, comfort and flexibility.
[0004] At present, shear thickening materials are mainly divided into the following two types:
[0005] (1) Shear thickening fluid: Shear thickening fluid is prepared by directly dispersing particles in a liquid. The particles are usually silica particles, and the liquid can be ethylene glycol, polyethylene glycol 200, etc. CN115071237A provides a composite film with a sandwich structure by placing a shear thickening fluid intermediate layer between two layers of polymer films. The composite film not only maintains the modulus, strength and flexibility of the polymer film itself, but also absorbs impact or vibration energy and thus has excellent toughness. CN114921083A discloses a polyurethane-polyurea double-layer shear thickening fluid microcapsule material, which can enhance the impact resistance of polymer materials and improve the processing fluidity of shear thickening fluid used in polymer composite materials. However, the use of shear thickening fluids often faces the following problems: ① It is difficult to evenly disperse the particles in the liquid matrix, resulting in reduced performance; ② Shear thickening fluids are liquids, and their unique rheological properties exist within a narrow concentration range, making them difficult to use in practical applications; ③ Shear thickening fluids are exposed to the air for a long time and easily absorb moisture in the air, thereby reducing their shear thickening performance; ④ Shear thickening fluids are often filled into porous materials when used, and once the porous materials are destroyed, the liquid is very easy to flow out; ⑤ The temperature requirements are relatively strict, and they are prone to fail at higher or lower temperatures.
[0006] (2) Shear-hardening gel: mainly refers to organic polyborosiloxane materials, which can deform freely at low shear rates. When the shear rate increases sharply, the material suddenly changes to show hard solid characteristics, the viscosity will rise sharply, and the system will undergo changes similar to phase transition. Shear-hardening gel overcomes many shortcomings of shear thickening liquid and has good thermal stability, which greatly expands the application prospects of shear thickening materials. CN105385163A provides a method for preparing a shear thickening gel-based shock-absorbing and energy-absorbing material. When the material is subjected to impact, the state will spontaneously change from soft to hard and absorb energy, thereby effectively playing a protective role. CN107474544A discloses a lightweight shear thickening gel, which uses hollow microspheres to modify traditional shear thickening gel, so that the overall weight of the shear thickening gel is light and the viscosity is reduced. When the same mass of shear thickening gel is applied to the sample, the protective effect of adding hollow microspheres is significantly enhanced. CN104862975A provides a method for preparing an anti-fragmentation fabric with a shear thickening effect, and the fabric has a good energy absorption effect. However, the current shear-hardening gels still have the following problems: ① Shear-hardening gels are limited by creep and have no fixed shape and cannot be used alone; ② Shear-hardening gels are immersed in traditional material forms, such as inert aramid fibers. Due to the poor bonding strength between the interface layers, interface failure is prone to occur, causing performance to decrease over time; ③ The effective shear-hardening gel volume ratio is too small to function.
[0007] Based on this, developing a new type of aerogel-based energy-absorbing material to overcome the shortcomings of existing shear thickening materials to meet the requirements of light weight, comfort, softness and good energy absorption performance in practical applications of protective materials is still an urgent problem to be solved. Summary of the invention
[0008] The main purpose of the present invention is to provide an aerogel-based energy absorbing material and a preparation method thereof, so as to overcome the deficiencies of the prior art.
[0009] Another object of the present invention is to provide a use of the aerogel-based energy absorbing material.
[0010] In order to achieve the aforementioned invention object, the present invention adopts the following technical solutions:
[0011] An embodiment of the present invention provides an aerogel-based energy absorbing material, which includes:
[0012] The porous aerogel material as a substrate includes a three-dimensional porous network structure formed by overlapping nanofibers and having interconnection;
[0013] And, energy-absorbing substances and selectively added or unadded functional additives loaded in the porous aerogel material, the functional additives can enhance the base material on the one hand, and introduce electrical conductivity, thermal conductivity and other properties to the base material on the other hand. The energy-absorbing substances and functional additives are wrapped on the nanofibers and embedded in the three-dimensional porous network structure. When the external strain rate or shear rate changes, the energy-absorbing substances can absorb and dissipate a large amount of impact energy, thereby protecting other materials or devices from damage. Wherein, the energy-absorbing substances include any one or a combination of two or more of polydimethylsiloxane, polyborosiloxane, soft and hard phase change materials, plasticine, natural rubber, chloroprene rubber, and nitrile rubber.
[0014] The embodiment of the present invention also provides a method for preparing the aforementioned aerogel-based energy absorbing material, which comprises:
[0015] Providing porous aerogel materials;
[0016] The energy absorbing material and the selectively added or unadded functional additives are filled into the porous aerogel material by in-situ polymerization or solution-assisted filling, and then dried to obtain the aerogel-based energy absorbing material.
[0017] The embodiment of the present invention also provides the application of the aerogel-based energy absorbing material in the fields of shock absorption and noise reduction, impact protection or energy absorption.
[0018] Compared with the prior art, the beneficial effects of the present invention are at least:
[0019] 1) The aerogel matrix structure used in the aerogel-based energy-absorbing material provided by the present invention can be individually designed, and the energy-absorbing material is freed from the limitations of creep and no fixed shape;
[0020] (2) The aerogel matrix used in the aerogel-based energy-absorbing material provided by the present invention has multiple active sites inside and on the surface, and the bonding strength between the interface layers is large;
[0021] (3) The aerogel matrix used in the aerogel-based energy-absorbing material provided by the present invention is composed of high-performance nanofibers, which can enhance the mechanical properties of the energy-absorbing material in the nano-confined region;
[0022] (4) The mass fraction of the energy absorbing substance in the aerogel-based energy absorbing material provided by the present invention can be as high as 99%, which is conducive to fully exerting the performance of the energy absorbing substance; at the same time, the preparation process is simple and easy to achieve large-scale production, and can be applied to the fields of shock absorption and noise reduction, impact protection, energy absorption, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 is a schematic structural diagram of an aerogel-based energy-absorbing material in a typical embodiment of the present invention;
[0025] Figure 2 is a thermogravimetric curve of the aramid aerogel film-based energy-absorbing material obtained in Example 1 of the present invention;
[0026] Figure 3 is an infrared spectrum of the aramid aerogel fiber-based energy-absorbing material obtained in Example 2 of the present invention;
[0027] Figure 4 is an optical photograph of the aramid aerogel honeycomb-based energy-absorbing material obtained in Example 3 of the present invention;
[0028] Figure 5 is an optical photograph of the cellulose aerogel film-based energy-absorbing material obtained in Example 4 of the present invention;
[0029] Figure 6 This is an optical photograph of the 3D printed cellulose aerogel lattice-based energy-absorbing material obtained in Example 5 of the present invention;
[0030] Figure 7 is a quasi-static stress-strain curve diagram of the cellulose aerogel block-based energy-absorbing material obtained in Example 6 of the present invention;
[0031] Figure 8 This is a photo showing the flexibility of the polyimide aerogel fiber-based energy-absorbing material obtained in Example 7 of the present invention;
[0032] Fig. 9 is an internal morphology diagram of the cellulose aerogel fiber-based energy-absorbing material obtained in Example 8 of the present invention;
[0033] Fig.10 This is a high-speed impact curve diagram of the silk protein aerogel film-based energy-absorbing material obtained in Example 9 of the present invention;
[0034] Fig.11 This is a high-speed impact curve diagram of the silver nanowire aerogel block-based energy-absorbing material obtained in Example 10 of the present invention. DETAILED DESCRIPTION
[0035] Shear-hardening gel has the following problems: ① Shear-hardening gel is limited by creep and has no fixed shape, so it cannot be used alone; ② Shear-hardening gel is immersed in traditional material forms, such as inert aramid fiber, and due to the poor bonding strength between the interface layers, it is easy to have interface failure, resulting in performance degradation over time; ③ The effective shear-hardening gel volume ratio is too small to play a role. These drawbacks make the protective performance of shear-hardening gel unable to meet the needs of practical applications.
[0036] In view of the deficiencies in the prior art, the inventor of this case, after long-term research and extensive practice, was able to propose the technical solution of the present invention, which mainly develops a new type of aerogel-based energy-absorbing material to overcome the deficiencies of the existing materials, so as to meet the requirements of light weight, comfort, and good energy absorption performance in the practical application of protective materials, and explains a series of applications of the aerogel-based energy-absorbing material. The technical solution, its implementation process and principle, etc. will be further explained as follows.
[0037] Specifically, as one aspect of the technical solution of the present invention, an aerogel-based energy absorbing material is involved, and its structure can be referred to as Figure 1 As shown, the aerogel-based energy-absorbing material is composed of a porous aerogel material substrate loaded with energy-absorbing substances and selectively added or unadded functional additives. The porous aerogel material has a designable specific arbitrary macroscopic morphological structure, and the interior is formed by overlapping nanofibers and has a connected three-dimensional porous network structure. The energy-absorbing substance and functional additives are wrapped on the nanofibers and embedded in the three-dimensional porous network structure.
[0038] Furthermore, the aerogel matrix used in the aerogel-based energy-absorbing material of the present invention is composed of high-performance nanofibers, which can enhance the mechanical properties of the energy-absorbing material in the nano-confined region. In addition, the aerogel matrix has multiple active sites inside and on the surface, and the bonding strength between the interface layers is large.
[0039] In some preferred embodiments, the types of the constituent unit nanofibers of the porous aerogel material include but are not limited to any one or a combination of two or more of aramid nanofibers, cellulose nanofibers, polyimide nanofibers, silk protein nanofibers, silver nanofibers, etc.
[0040] In some preferred embodiments, the macroscopic structure of the porous aerogel material includes, but is not limited to, any one or a combination of two or more of a honeycomb, a crisscross pattern, a three-dimensional lattice, a film, a fiber, a block, and the like.
[0041] In some preferred embodiments, the porous aerogel material has a hierarchical porous network structure, which is composed of micropores with a pore size of less than 2nm, mesopores with a pore size of 2nm to 50nm, and macropores with a pore size of 50nm to 10cm. The porosity of the porous aerogel material is 50 to 99.99%, and the density is 0.1 to 1500mg / cm 3 , with a specific surface area of 50 to 2500m 2 / g, pore volume is 0.1~15cm 3 / g.
[0042] Furthermore, when the external strain rate or shear rate changes, the energy absorbing material can absorb and dissipate a large amount of impact energy, thereby protecting other materials or devices from damage.
[0043] In some preferred embodiments, the energy absorbing material includes but is not limited to any one or a combination of two or more of polydimethylsiloxane, polyborosiloxane, soft and hard phase change materials, plasticine, natural rubber, chloroprene rubber, nitrile rubber, etc.
[0044] In some preferred embodiments, the content of the energy absorbing substance in the aerogel-based energy absorbing material is 30wt% to 99wt%. The mass fraction of the energy absorbing substance in the aerogel-based energy absorbing material of the present invention can be as high as 99%, which is conducive to fully exerting the performance of the energy absorbing substance.
[0045] In some preferred embodiments, the functional additives include but are not limited to any one or a combination of two or more of calcium carbonate, carbon nanotubes, graphene, transition metal nitrides / carbides (MXene), metals (such as gold nanoparticles), silicon dioxide particles, etc. Further, the functional additives can enhance the base material on the one hand, and introduce electrical conductivity, thermal conductivity and other properties to the base material on the other hand.
[0046] Furthermore, the content of the functional additive in the aerogel-based energy-absorbing material is 0wt% to 30wt%.
[0047] In some preferred embodiments, the energy absorption value of the aerogel-based energy absorbing material is 0.1 to 1000 J / g.
[0048] Another aspect of an embodiment of the present invention provides a method for preparing an aerogel-based energy absorbing material, which comprises:
[0049] Providing porous aerogel materials;
[0050] The energy absorbing material and the selectively added or unadded functional additives are filled into the porous aerogel material by in-situ polymerization or solution-assisted filling, and then dried to obtain the aerogel-based energy absorbing material.
[0051] In some preferred embodiments, the preparation method specifically comprises:
[0052] (1) Selecting a porous aerogel material with a specific macrostructure and super strong capillary force as the substrate;
[0053] (2) Introducing energy-absorbing substances and functional additives into the three-dimensional porous network structure of porous aerogel materials by in-situ polymerization or solution-assisted filling;
[0054] (3) removing excess energy-absorbing material on the surface and drying the material to obtain an aerogel-based composite energy-absorbing material with high energy absorption.
[0055] In some specific embodiments, the method for preparing the porous aerogel material includes: preparing the porous aerogel material by at least one or more of a combination of wet spinning, confined sol-gel reaction spinning, freeze-drying spinning, template method, 3D printing method, and scraping method, but is not limited thereto.
[0056] In some specific embodiments, the drying includes at least any one of freeze drying, vacuum drying or normal pressure drying, but is not limited thereto.
[0057] In some specific embodiments, the in-situ polymerization method includes: placing an energy absorbing material prepolymer in a reaction container and making it contact with a porous aerogel material, letting it stand for 1 hour to 24 hours, taking out and removing excess energy absorbing material prepolymer on the surface, then polymerizing the energy absorbing material prepolymer in situ, and then drying to obtain an aerogel-based energy absorbing material.
[0058] Furthermore, the energy absorbing material prepolymer may include an energy absorbing material precursor (such as a soft and hard phase change material prepolymer benzyl methacrylate monomer), an initiator (such as a 1-hydroxycyclohexyl phenyl ketone photoinitiator), a crosslinker (such as ethylene glycol dimethacrylate) and an ionic liquid (such as 1-ethyl-3-methylimidazole bistrifluoromethanesulfonyl imide salt).
[0059] Furthermore, the energy absorbing material prepolymer may also include an energy absorbing material precursor (such as chloroprene monomer), an emulsifier (such as rosin acid soap emulsifier), an initiator (such as potassium persulfate), a relative molecular weight regulator (such as n-dodecyl mercaptan), a vulcanizing agent (such as sulfur) and a solvent (such as water), but is not limited thereto.
[0060] Furthermore, the in-situ polymerization method specifically includes the following steps:
[0061] The energy absorbing material prepolymer is placed in a container, and the porous aerogel material is immersed therein, and the container is left to stand for 1 hour to 24 hours. The excess energy absorbing material prepolymer on the surface is taken out and removed, and then the container is placed in a specific environment to polymerize the energy absorbing material prepolymer in situ, and then freeze-dried, vacuum-dried or dried at normal pressure to obtain an aerogel-based energy absorbing material.
[0062] In some specific embodiments, the solution-assisted filling method includes: dissolving the energy-absorbing material in a selected solvent to form an energy-absorbing material solution, wherein the concentration of the energy-absorbing material solution is 1wt% to 60wt%; and contacting the porous aerogel material with the energy-absorbing material solution, standing for 1h to 24h, taking out and removing the energy-absorbing material on the surface, and then drying to obtain an aerogel-based energy-absorbing material.
[0063] Furthermore, the solution-assisted filling process specifically includes the following steps:
[0064] The energy absorbing material is dissolved in a selected solvent, and the porous aerogel material is immersed in the energy absorbing material solution, and allowed to stand for 1 hour to 24 hours, and the surface energy absorbing material solution is taken out and removed, and the aerogel-based energy absorbing material is obtained after freeze drying, vacuum drying or normal pressure drying.
[0065] Furthermore, the selected solvent includes but is not limited to any one or a combination of two or more of water, cyclohexane, ethanol, tert-butanol, acetone, tetrahydrofuran, ethyl acetate, etc.
[0066] The aerogel-based energy-absorbing material of the present invention can be prepared into any size and shape, and the structure is designable, and the energy-absorbing material is free from the limitations of creep and no fixed shape; and can be cut according to different sizes and coated on irregular surfaces. At the same time, the preparation process is simple, the conditions are mild and controllable, and it is easy to achieve large-scale production.
[0067] Another aspect of the embodiments of the present invention further provides the application of the aforementioned aerogel-based energy absorbing material in the fields of shock absorption and noise reduction, impact protection, energy absorption, etc.
[0068] In summary, through the above technical scheme, the aerogel-based energy-absorbing material provided by the present invention is composed of a porous aerogel matrix loaded with energy-absorbing substances and functional additives. The porous aerogel matrix is formed by overlapping nanofibers, has a continuous three-dimensional porous network structure, has an adjustable macrostructure, density, porosity, specific surface area, etc., and has a strong capillary force. The energy-absorbing substances and functional additives are adsorbed on the surface and pores of the nanofibers of the porous aerogel matrix. The aerogel-based energy-absorbing material has high energy absorption and high sensitivity, and has a very broad application prospect. It can be used in the fields of shock absorption and noise reduction, impact protection, energy absorption, etc.
[0069] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention is further described in detail in combination with several preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, and those skilled in the art can make adjustments according to actual conditions. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention. For the test methods in the following embodiments that do not specify specific conditions, the test methods in the embodiments are all carried out under normal conditions. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0070] Example 1
[0071] This embodiment provides an aramid aerogel film-based energy-absorbing material, and a preparation method thereof comprises the following steps:
[0072] (1) Preparation of aramid aerogel film: A 0.5 wt % aramid nanofiber dispersion was prepared and an aramid aerogel film was prepared by a doctor blade coating method.
[0073] (2) Preparation of filling material: prepare a polyborosiloxane / anhydrous ethanol solution with a mass fraction of 30 wt%.
[0074] (3) Preparation of aramid aerogel film-based energy-absorbing material: Place the aramid nanofiber aerogel film in the aforementioned solution, take it out after standing for 12 hours, remove the excess polyborosiloxane / anhydrous ethanol solution on the surface, dry it at normal pressure, and obtain an aerogel-based composite energy-absorbing film.
[0075] Figure 2 3 is the thermogravimetric curve of the aramid aerogel film-based energy-absorbing material obtained in Example 1. For other parameters, please refer to Table 1.
[0076] Example 2
[0077] This embodiment provides an aramid aerogel fiber-based energy-absorbing material, and a preparation method thereof comprises the following steps:
[0078] (1) Preparation of aramid aerogel fibers: A 10 wt % aramid nanofiber dispersion was prepared and aramid aerogel fibers were prepared by wet spinning.
[0079] (2) Preparation of filling material: prepare a polyborosiloxane / tert-butyl alcohol solution with a mass fraction of 60 wt%.
[0080] (3) Preparation of aramid aerogel fiber-based energy-absorbing material: Aramid nanofiber aerogel fibers were placed in the aforementioned solution, allowed to stand for 1 hour, and then taken out to remove excess polyborosiloxane / tert-butyl alcohol solution on the surface, and vacuum dried to obtain aerogel-based composite energy-absorbing fibers.
[0081] Figure 3 : is the infrared spectrum of the aramid aerogel fiber-based energy-absorbing material obtained in Example 2. For other parameters, please refer to Table 1.
[0082] Example 3
[0083] This embodiment provides an aramid aerogel honeycomb-based energy-absorbing material, and a preparation method thereof comprises the following steps:
[0084] (1) Preparation of aramid aerogel honeycomb: A 5 wt % aramid nanofiber dispersion was prepared and an aramid aerogel honeycomb was prepared using a template method.
[0085] (2) Preparation of filling material: A 10 wt % plasticine / cyclohexane solution was prepared, and 5 wt % of gold nanoparticles were added as a functional additive.
[0086] (3) Preparation of aramid aerogel honeycomb-based energy-absorbing material: Place the aramid nanofiber aerogel honeycomb in the aforementioned solution, let it stand for 24 hours, then take it out, remove the excess filling liquid on the surface, and vacuum dry it to obtain an aramid aerogel-based composite energy-absorbing honeycomb.
[0087] Figure 4 This is an optical photograph of the aramid aerogel honeycomb-based energy-absorbing material obtained in Example 3. For other parameters, please refer to Table 1.
[0088] Example 4
[0089] This embodiment provides a cellulose aerogel film-based energy-absorbing material, and the preparation method thereof comprises the following steps:
[0090] (1) Preparation of cellulose aerogel film: A 0.1 wt % cellulose nanofiber dispersion was prepared and a cellulose aerogel film was prepared by a doctor blade coating method.
[0091] (2) Preparation of filling material: prepare a polyborosiloxane / acetone solution with a mass fraction of 10 wt%, and add 10 wt% of silicon dioxide powder as a functional additive.
[0092] (3) Preparation of cellulose aerogel film-based energy-absorbing material: Place the cellulose nanofiber aerogel film in the aforementioned energy-absorbing material, let it stand for 8 hours, then take it out, remove the excess material on the surface, and vacuum dry it to obtain an aerogel-based composite energy-absorbing film.
[0093] Figure 5 This is an optical photograph of the cellulose aerogel film-based energy-absorbing material obtained in Example 4. For other parameters, please refer to Table 1.
[0094] Example 5
[0095] This embodiment provides a 3D printed cellulose aerogel three-dimensional lattice-based energy-absorbing material, and the preparation method thereof comprises the following steps:
[0096] (1) Preparation of 3D printed cellulose aerogel three-dimensional lattice: A 2 wt% cellulose nanofiber dispersion was prepared, and a 3D printed cellulose aerogel three-dimensional lattice structure was prepared by a direct writing 3D printing method.
[0097] (2) Preparation of filling material: Mix the soft and hard phase change material prepolymer benzyl methacrylate monomer, 1-hydroxycyclohexyl phenyl ketone photoinitiator, ethylene glycol dimethacrylate crosslinker, 1-ethyl-3-methylimidazole bistrifluoromethanesulfonyl imide salt, 30wt% calcium carbonate powder, etc. evenly.
[0098] (3) Preparation of 3D printed cellulose aerogel stereo lattice-based energy-absorbing material: The 3D printed cellulose aerogel stereo lattice was placed in the aforementioned mixed solution, taken out after standing for 6 hours, and the excess material on the surface was removed. The material was then placed under ultraviolet light for curing for 10 hours to obtain an aerogel-based composite energy-absorbing material.
[0099] Figure 6 This is an optical photograph of the 3D printed cellulose aerogel lattice-based energy-absorbing material obtained in Example 5. For other parameters, please refer to Table 1.
[0100] Example 6
[0101] This embodiment provides a cellulose aerogel block-based energy absorbing material, and the preparation method thereof comprises the following steps:
[0102] (1) Preparation of cellulose aerogel blocks: 8 wt % cellulose nanofiber dispersion was prepared and cellulose aerogel blocks were prepared by direct freeze drying.
[0103] (2) Preparation of filling material: Chop the nitrile rubber into pieces and prepare a 10 wt% nitrile rubber / ethyl acetate solution, then add 1 wt% of graphene additive and stir evenly.
[0104] (3) Preparation of cellulose aerogel block-based energy-absorbing material: Place the cellulose nanofiber aerogel block in the aforementioned mixed solution, let it stand for 1 hour, then take it out, remove the excess material on the surface, wash it, and then place the material in a 90°C oven for 15 hours to obtain an aerogel-based composite energy-absorbing block.
[0105] Figure 7 : This is the quasi-static stress-strain curve of the cellulose aerogel block-based energy-absorbing material obtained in Example 6. For other parameters, please refer to Table 1.
[0106] Example 7
[0107] This embodiment provides a polyimide aerogel fiber-based energy-absorbing material, and the preparation method thereof comprises the following steps:
[0108] (1) Preparation of polyimide aerogel fibers: Polyimide aerogel fibers with a solid content of 10 wt% were prepared by confined spinning.
[0109] (2) Preparation of filling material: Chop the natural rubber into small pieces and prepare a natural rubber / tetrahydrofuran solution with a mass fraction of 10 wt%.
[0110] (3) Preparation of polyimide aerogel fiber-based energy-absorbing material: The polyimide aerogel fiber was placed in the aforementioned mixed solution, allowed to stand for 6 hours, and then taken out to remove excess surface material and wash. The material was then placed in a 90°C oven for 15 hours to obtain an aerogel-based composite energy-absorbing block.
[0111] Figure 8 This is a photo showing the flexibility of the polyimide aerogel fiber-based energy-absorbing material obtained in Example 7. For other parameters, please refer to Table 1.
[0112] Example 8
[0113] This embodiment provides a cellulose aerogel fiber-based energy-absorbing material, and the preparation method thereof comprises the following steps:
[0114] (1) Preparation of cellulose aerogel fibers: A 0.1 wt % cellulose nanofiber dispersion was prepared and cellulose aerogel fibers were prepared by wet spinning.
[0115] (2) Preparation of filling material: sulfur vulcanizing agent and rosin acid soap emulsifier are added to chloroprene to prepare an oil phase; water and sodium hydroxide are prepared to prepare an aqueous phase; then, after the oil phase and the aqueous phase are emulsified, n-dodecyl mercaptan relative molecular weight regulator and potassium persulfate initiator solution are added, and the system is stirred evenly in an ice bath at 4°C.
[0116] (3) Preparation of cellulose aerogel fiber-based energy-absorbing material: Cellulose nanofiber aerogel fibers were placed in the aforementioned mixed solution, allowed to stand for 10 min, and then taken out to remove excess surface material. The material was then placed in a 40°C environment for 3 h, cooled, and subjected to chain termination, coagulation, washing, and normal pressure drying to obtain an aerogel-based composite energy-absorbing fiber.
[0117] Fig. 9 This is the internal morphology of the cellulose aerogel fiber-based energy-absorbing material obtained in Example 8. For other parameters, please refer to Table 1.
[0118] Example 9
[0119] This embodiment provides a silk protein aerogel film-based energy-absorbing material, and the preparation method thereof comprises the following steps:
[0120] (1) Preparation of silk fibroin aerogel film: A 0.5 wt % silk fibroin nanofiber dispersion was prepared and a silk fibroin aerogel film was prepared by a doctor blade coating method.
[0121] (2) Preparation of filling material: After preparing a polydimethylsiloxane / anhydrous ethanol solution with a mass fraction of 1 wt%, 1 wt% of carbon nanotubes was added.
[0122] (3) Preparation of silk protein aerogel film-based energy-absorbing material: Place the silk protein nanofiber aerogel film in the aforementioned solution, take it out after standing for 12 hours, remove the excess polydimethylsiloxane / anhydrous ethanol solution on the surface, dry it at normal pressure, and obtain an aerogel-based composite energy-absorbing film.
[0123] Fig.10 This is the high-speed impact curve of the silk protein aerogel film-based energy-absorbing material obtained in Example 9. For other parameters, please refer to Table 1.
[0124] Example 10
[0125] This embodiment provides a silver nanowire aerogel block-based energy absorbing material, and the preparation method thereof comprises the following steps:
[0126] (1) Preparation of silver nanowire aerogel blocks: 10 wt % silver nanowire dispersion was prepared, and silver nanowire aerogel blocks were prepared by direct drying method.
[0127] (2) Preparation of filling material: Prepare a 20 wt% polydimethylsiloxane / anhydrous ethanol solution and add 1 wt% transition metal nitride / carbide (Ti3C2T x MXene).
[0128] (3) Preparation of silver nanowire aerogel film-based energy-absorbing material: The silver nanowire aerogel film was placed in the aforementioned solution, and after standing for 12 hours, it was taken out to remove the excess polydimethylsiloxane / anhydrous ethanol solution on the surface, followed by washing and freeze-drying to obtain an aerogel-based composite energy-absorbing block.
[0129] Fig.11 This is the high-speed impact curve of the silver nanowire aerogel block-based energy-absorbing material obtained in Example 10. For other parameters, please refer to Table 1.
[0130] Table 1 Energy absorption values of aerogel-based energy absorbing materials obtained in Examples 1-10
[0131]
[0132]
[0133] Comparative Example 1
[0134] This comparative example provides an aramid aerogel film material, and compared with Example 1, this comparative example does not add the polyborosiloxane / anhydrous ethanol solution. The energy absorption value of the obtained material is 30 J / g.
[0135] Through Examples 1-10, it can be found that the aerogel-based energy-absorbing material obtained by the above technical solution of the present invention has excellent properties such as designable structure, high load capacity, excellent energy absorption effect, and simple process.
[0136] In addition, the inventors of this case also conducted experiments with other raw materials and conditions listed in this specification in accordance with the methods of Examples 1-10, and also produced aerogel-based energy-absorbing materials with designable structure, high load capacity, excellent energy absorption effect and wide application.
[0137] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made and that elements of the described embodiments may be substituted with substantial equivalents without departing from the spirit and scope of the present invention. In addition, many modifications may be made to adapt a particular situation or material to the teachings of the present invention without departing from the scope of the present invention. Therefore, it is not intended herein to limit the present invention to the specific disclosed embodiments for carrying out the present invention, but rather it is intended that the present invention will include all embodiments within the scope of the appended claims.
Claims
1. An aerogel-based energy-absorbing material, characterized in that: include: The porous aerogel material as a substrate includes a three-dimensional porous network structure formed by overlapping nanofibers and having interconnection; And, energy-absorbing substances and functional additives loaded in the porous aerogel material, the energy-absorbing substances and functional additives are wrapped on the nanofibers and embedded in the three-dimensional porous network structure, wherein the energy-absorbing substances are selected from any one or a combination of two or more of polydimethylsiloxane, polyborosiloxane, plasticine, natural rubber, chloroprene rubber, and nitrile rubber, and the functional additives are selected from any one or a combination of two or more of calcium carbonate, carbon nanotubes, graphene, transition metal nitrides, transition metal carbides, metals, and silica particles. The content of the energy-absorbing substance in the aerogel-based energy-absorbing material is 30 wt%~99 wt%, and the content of the functional additive in the aerogel-based energy-absorbing material is 1 wt%~30 wt%.
2. The aerogel-based energy absorbing material according to claim 1, characterized in that: The nanofiber is selected from any one or a combination of two or more of aramid nanofiber, cellulose nanofiber, polyimide nanofiber, silk protein nanofiber, and silver nanofiber; And / or, the macroscopic structure of the porous aerogel material is selected from any one or a combination of two or more of a honeycomb, a crisscross pattern, a three-dimensional lattice, a film, a fiber, and a block; And / or, the porous aerogel material has a hierarchical porous network structure inside, which is composed of micropores with a pore size of less than 2 nm, mesopores with a pore size of 2 nm to 50 nm, and macropores with a pore size of 50 nm to 10 cm. The porosity of the porous aerogel material is 50 to 99.99%, and the density is 0.1 to 1500 mg / cm 3 , with a specific surface area of 50~2500 m 2 / g, pore volume is 0.1~15 cm 3 / g.
3. The aerogel-based energy absorbing material according to claim 1, characterized in that: The energy absorption value of the aerogel-based energy absorbing material is 0.1-1000 J / g.
4. The method for preparing an aerogel-based energy-absorbing material according to any one of claims 1 to 3, characterized in that: include: Providing porous aerogel materials; The energy absorbing material and functional additives are filled into the porous aerogel material by in-situ polymerization or solution-assisted filling, and then dried to obtain an aerogel-based energy absorbing material.
5. The preparation method according to claim 4, characterized in that: include: The porous aerogel material is prepared by at least one or more of a combination of wet spinning, confined sol-gel reaction spinning, freeze-drying spinning, template method, 3D printing method, and blade coating method.
6. The preparation method according to claim 4, characterized in that include: The energy absorbing material is dissolved in a selected solvent to form an energy absorbing material solution, and the porous aerogel material is brought into contact with the energy absorbing material solution, and allowed to stand for 1 h to 24 h, the energy absorbing material on the surface is taken out and removed, and then dried to obtain an aerogel-based energy absorbing material.
7. The preparation method according to claim 6, characterized in that: The concentration of the energy absorbing material solution is 1 wt% to 60wt%.
8. The preparation method according to claim 6, characterized in that: The selected solvent is selected from any one of water, cyclohexane, ethanol, tert-butanol, acetone, tetrahydrofuran, and ethyl acetate, or a combination of two or more thereof.
9. The preparation method according to claim 4, characterized in that: The drying is selected from at least any one of freeze drying, vacuum drying or normal pressure drying.
10. Use of the aerogel-based energy absorbing material according to any one of claims 1 to 3 in the field of vibration reduction, noise reduction or energy absorption.