A kind of Bi x Se y / C composite material, preparation method and application thereof, and method for regulating bismuth-selenium atomic ratio of the composite material
Patent Information
- Application Number
- CN202211002695.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-08-19
AI Technical Summary
[0003]目前,针对硒化铋基电极材料的研究虽然已经取得了一定进展,但仍然不够完善,整体处于初期阶段,主要是由于以下问题尚未解决,难以取得进一步突破:
[0042] In the present invention, the bismuth/carbon composite material is prepared by directly calcining the organic bismuth salt, and then mixed with selenium element and calcined again to obtain Bi x Se y /C composite material, Bi in this composite material x Se y The nanodots are evenly embedded in the sheet-like carbon skeleton, and the Bi x Se y Nanodots can shorten the ion diffusion distance, and the carbon skeleton can improve Bi x Se y The conductivity between nanodots forms a tight electronic connection. On the other hand, it can enhance the mechanical stress of the composite material and build a fast and stable transmission channel, thus forming an overall efficient ion/electron transmission network to ensure the electrolyte and electrode Full contact between materials is conducive to M + (M=Li, Na, K) and rapid transmission of electrons to achieve rapid reaction dynamics. Applying this composite material as an electrode material can exhibit ultra-long cycle life and excellent rapid M storage capability.
Smart Images

Figure CN115763715B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrode materials, and more specifically, to a Bi x Se y / C composite material, preparation method and application thereof, and method for regulating the atomic ratio of bismuth and selenium in the composite material. Background Art
[0002] Bismuth selenide (Bi x Se y )-based materials, such as BiSe, BiSe2, Bi3Se2, Bi4Se3 and Bi3Se4, have been considered to have great potential in optics and modern thermoelectrics. In recent years, with the rapid development of lithium / sodium ion batteries, bismuth selenide (BiSe) has been widely used in the research of optics and modern thermoelectrics. x Se y ) materials have a unique layered crystal structure, conversion-alloy energy storage mechanism and relatively small shuttle effect. They are also considered to have the potential to achieve higher reversible capacity, faster reaction kinetics and more stable cycle performance, and thus have begun to receive widespread attention in the field of electrochemistry.
[0003] At present, although some progress has been made in the research on bismuth selenide-based electrode materials, it is still not perfect and is still in its early stages. This is mainly because the following problems have not been solved, making it difficult to make further breakthroughs:
[0004] (1) Like other alloy / conversion mechanism electrode materials, on the one hand, bismuth selenide-based electrode materials have a dramatic volume expansion, which can easily lead to electrode crushing and rupture, and rapid capacity decay. At the same time, the incomplete reversibility of the conversion reaction will also lead to continuous capacity decay. The common strategy to address this problem is to construct a sophisticated and stable composite structure to provide sufficient buffer space, but its preparation process is complex, costly, and has a low yield, making it difficult to achieve practical application;
[0005] (2) Bismuth selenide is a typical semiconductor, and its inherent low conductivity severely limits its rate performance. To address this problem, doping and carbon coating strategies are often used to improve its conductivity. For example, Li et al. used a solvothermal method and obtained a Bi-MOFs precursor by washing and drying with an organic solvent, and then prepared N-doped carbon-coated Bi2Se3 / NC composites after high-temperature calcination with selenium powder (Ceramics International, 2019, 45, 11861–11867, DOI: 10.1016 / j.ceramint.2019.03.068); Jin et al. combined organic solvothermal method with high-temperature calcination to prepare CNTs@C@Bi2Se3 composites with carbon double coating (Ceramics International, 2017, 43, 17093–17099, DOI: 10.1016 / j.ceramint.2017.09.124). However, due to the weak heterogeneous interface connection in traditional carbon coating, it is difficult to form a close electronic connection, so it is difficult to fully utilize the potential of carbon carriers. The N-doped carbon-coated Bi2Se3 / NC composites prepared by Li et al. -1 After 400 cycles at the current density, the capacity is only 335.8 mAh g -1 (Ceramics International, 2019, 45, 11861–11867, DOI: 10.1016 / j.ceramint.2019.03.068); while the maximum rate of the carbon nanotube-carbon double-coated CNTs@C@Bi2Se3 composite prepared by Jin et al. is only 2A g -1 , and at 1A g -1 After 300 cycles at the same current density, the capacity can only be retained at 243 mAh g -1 (Ceramics International, 2017, 43, 17093–17099, DOI: 10.1016 / j.ceramint.2017.09.124).
[0006] (3) At present, the research on bismuth selenide-based electrode materials is only focused on Bi2Se3. In fact, Bi with different atomic ratios x Se yBi-based materials often exhibit different crystal structures and physicochemical properties, resulting in different morphological structures and surface properties, which affect the performance of electrode materials. In addition, the capacity contribution of alloying and conversion reactions in bismuth selenide-based materials is closely related to the Bi:Se atomic ratio. Theoretically, as the Bi content increases, the proportion of highly reversible alloy reactions increases, and the overall reversibility improves, but the additional capacity brought by the conversion process will decrease, resulting in a decrease in theoretical capacity. Therefore, the continuous development of different preparation methods for different types of Bi is needed. x Se y It is very necessary to adjust the Bi:Se atomic ratio of the base material to achieve the best balance between specific capacity and reversibility, which can further optimize the bismuth selenide electrode material system and expand its development and application. Summary of the invention
[0007] Based on the above technical problems existing in the prior art, one of the purposes of the present invention is to provide a Bi x Se y A method for preparing a Bi / C composite material, wherein the Bi x Se y The nanodots are uniformly embedded in the flaky carbon skeleton, constructing a stable C-Se interface chemical bond, improving material stability and accelerating ion transport, while also increasing Bi x Se y The mechanical stress of the crystal structure of the / C composite material not only shortens the ion diffusion distance but also ensures a sufficient buffer zone to improve the stability of the composite material structure.
[0008] In order to achieve the above object, the technical solution of the present invention is as follows:
[0009] A kind of Bi x Se y A method for preparing a / C composite material comprises the following steps:
[0010] Step S1, directly calcining the organic bismuth salt to obtain a bismuth / carbon precursor material;
[0011] Step S2: Mix the bismuth / carbon precursor material with selenium and calcine again to obtain Bi x Se y / C composite materials;
[0012] Among them, x=1~4, y=1~4.
[0013] In some embodiments, in step S2, the calcination temperature is 600-1000°C, preferably 600-900°C.
[0014] In some embodiments, in step S2, the heating rate is 2-5°C / min, preferably 3°C / min.
[0015] In some embodiments, in step S2, the calcination time is 2 to 3 hours, preferably 2 hours.
[0016] In some embodiments, the organic bismuth salt is at least one of bismuth citrate, bismuth subsalicylate, bismuth neodecanoate, bismuth subgallate, bismuth isooctanoate, bismuth laurate, and bismuth cyclohexaneate. Preferably, the organic bismuth salt is bismuth citrate (C6H5BiO7).
[0017] In some embodiments, in step S2, the mass ratio of the bismuth / carbon precursor material to the selenium element is 1:1.5-3; preferably, the mass ratio of the two is 1:2.
[0018] In some embodiments, in both step S1 and step S2, calcination is performed under an inert atmosphere, which includes an argon atmosphere, a helium atmosphere, a nitrogen atmosphere, a neon atmosphere, etc. Preferably, the inert atmosphere is an argon atmosphere.
[0019] In some embodiments, in step S1, the calcination temperature is 800-1000°C.
[0020] In some embodiments, in step S1, the heating rate is 2-8°C / min, preferably 5°C / min.
[0021] In some embodiments, in step S1, the calcination time is 3 to 5 hours, preferably 3 hours.
[0022] The second object of the present invention is to provide Bi prepared by the preparation method of any of the above embodiments. x Se y / C composite material.
[0023] The third object of the present invention is to provide a Bi x Se y / C composite electrode materials.
[0024] A fourth object of the present invention is to provide a negative electrode comprising the above-mentioned electrode material.
[0025] A fifth object of the present invention is to provide an alkali metal ion electrochemical energy storage device comprising the above-mentioned negative electrode.
[0026] In some embodiments, the alkali metal ion electrochemical energy storage includes but is not limited to lithium ion batteries, sodium ion batteries, potassium ion batteries, lithium ion capacitors, sodium ion capacitors, potassium ion capacitors, etc.
[0027] The sixth object of the present invention is to provide a method for regulating Bi x Se y The method for the atomic ratio of bismuth and selenium in a C / C composite material comprises the following steps:
[0028] Step 1: directly calcining the organic bismuth salt to obtain a bismuth / carbon precursor material;
[0029] Step 2: Mix the bismuth / carbon precursor material with selenium and calcine it again to obtain Bi x Se y / C composite materials;
[0030] Wherein, x=1~4, y=1~4;
[0031] The Bi x Se y In the Bi / C composite material, the x Se y Embedded in a sheet-like carbon skeleton.
[0032] In some embodiments, in step S1, the calcination temperature is 800-1000°C.
[0033] In some embodiments, in step S1, the heating rate is 2-8°C / min, preferably 5°C / min.
[0034] In some embodiments, in step S1, the calcination time is 3 to 5 hours, preferably 3 hours.
[0035] In some embodiments, in step S2, the calcination temperature is 600-1000°C.
[0036] In some embodiments, in step S2, the heating rate is 2-5°C / min, preferably 3°C / min.
[0037] In some embodiments, in step S2, the calcination time is 2 to 3 hours, preferably 2 hours.
[0038] In some embodiments, the organic bismuth salt is at least one of bismuth citrate, bismuth subsalicylate, bismuth neodecanoate, bismuth subgallate, bismuth isooctanoate, bismuth laurate, and bismuth cyclohexaneate.
[0039] In some embodiments, in step S2, the mass ratio of the bismuth / carbon precursor material to the selenium element is 1:1.5-3; preferably, the mass ratio of the two is 1:2.
[0040] In some embodiments, in both step S1 and step S2, calcination is performed under an inert atmosphere, which includes an argon atmosphere, a helium atmosphere, a nitrogen atmosphere, a neon atmosphere, etc. Preferably, the inert atmosphere is an argon atmosphere.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] The present invention directly calcines an organic bismuth salt to prepare a bismuth / carbon composite material, and then mixes it with a single substance of selenium and calcines it again to obtain a Bi x Se y / C composite material, in which Bi x Se y The nanodots are evenly embedded in the flake carbon skeleton, and the Bi x Se y Nanodots can shorten the ion diffusion distance, and the carbon skeleton can improve Bi x Se y On the one hand, it can enhance the conductivity between the nanodots, form a close electronic connection, and on the other hand, it can enhance the mechanical stress of the composite material and build a fast and stable transmission channel, thereby forming an efficient ion / electron transmission network as a whole, ensuring full contact between the electrolyte and the electrode material, which is beneficial to M + (M=Li, Na, K) and the rapid transmission of electrons realizes rapid reaction kinetics. The composite material can be used as an electrode material to show an ultra-long cycle life and excellent rapid M storage capacity.
[0043] In the process of preparing the composite material, the present invention can induce the formation of an interface C-Se bond, thereby reducing the M + Migrate the energy barrier to speed up ion transport and narrow the band gap to effectively enhance its conductivity, thereby speeding up electron transport.
[0044] The regulation Bi provided by the present invention x Se y The method for the bismuth-selenium atomic ratio in the bismuth-carbon composite material can be achieved by adjusting the reaction temperature during the reaction between the bismuth-carbon precursor material and the selenium element. x Se y The atomic ratio of bismuth and selenium in the / C composites and the x Se y The spacing between nanodots can be controlled to obtain a series of Bi with different morphologies and structures and different physical and chemical properties. x Se y / C composite materials. The preparation process of this method is simple and the regulation effect is significant. It is an important breakthrough in bismuth selenide-based electrode materials and provides new guidance and new ideas for subsequent diversified development. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 is the XRD pattern of each composite material in Examples 1, 2 and 3;
[0046] Figure 2 TEM image of the Bi3Se4 / C composite material in Example 1;
[0047] Figure 3 This is a graph showing the rate performance of a lithium-ion battery of the Bi3Se4 / C composite material in Example 1;
[0048] Figure 4 This is a graph showing the rate performance of the sodium ion battery of the Bi3Se4 / C composite material in Example 1;
[0049] Figure 5 TEM image of the Bi2Se3 / C composite material in Example 2;
[0050] Figure 6 This is a graph showing the rate performance of a lithium-ion battery of the Bi2Se3 / C composite material in Example 2;
[0051] Figure 7 TEM image of the Bi4Se3 / C composite material in Example 3;
[0052] Figure 8 This is a graph of the lithium-ion battery rate performance of the Bi4Se3 / C composite material in Example 3. DETAILED DESCRIPTION
[0053] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.
[0054] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0055] Example 1
[0056] (I) Preparation of precursor
[0057] Bismuth citrate was heated at 5 °C min in an argon atmosphere. -1 The precursor bismuth / carbon composite material (Bi / C) was obtained by heating to 900°C at a heating rate of and calcining for 3 hours.
[0058] (II) Preparation of Bi3Se4 / C composite materials
[0059] The Bi / C precursor and selenium powder were ground into uniform powder in a mass ratio of 1:2, and the obtained uniform mixture was placed in a tube furnace and heated at 3 °C min-1 under an argon atmosphere. -1 The temperature was raised to 800°C at a heating rate and the selenization calcination was carried out for 2 hours. Finally, the black product was collected after cooling to room temperature. The XRD test results are as follows: Figure 1 As shown, through Figure 1 The XRD results show that the product is a Bi3Se4 / C composite material. Figure 1 As shown in the transmission electron microscopy image of Figure 2 It is shown that the composite material is a composite structure in which Bi3Se4 nanodots are uniformly embedded in a flaky carbon skeleton.
[0060] The Bi3Se4 / C composite material prepared above was made into a negative electrode. Specifically, the prepared Bi3Se4 / C composite material was mixed with Super P (conductive agent) and sodium carboxymethyl cellulose (CMC, binder) in a mass ratio of 70:15:15, and an appropriate amount of deionized water was added to prepare a slurry, which was then coated on the current collector copper foil by a coating method, and after the deionized water evaporated, it was vacuum dried at 80°C for 12 hours. The copper foil containing the active material was cut into discs with a diameter of 14 mm, and was pressed under a pressure of 10 MPA, and then transferred to an inert gas glove box.
[0061] In an Ar atmosphere glove box, lithium metal was used as the counter electrode, LiPF6 / EC:DMC:DEC=1:1:1 (5% FEC) was used as the electrolyte, and Celgard 2400 membrane was used as the separator to assemble a CR2016 button cell. The electrochemical performance test was then carried out for lithium-ion batteries. -1 At the current density, it maintains 607.4 mAh g after 200 cycles. -1 Capacity; at 0.5A g -1 At the current density, it maintains 616.4 mAh g after 600 cycles. -1 Capacity; at 2A g -1 At the current density, it maintains 392 mAh g after 1500 cycles. -1 The capacity of Figure 2 As shown, at 0.1, 0.2, 0.5, 1, 2, 5, 10, 15 and 20A g -1 At current densities of 1.3, 1.7, 2.1, 3.3, 5.9, 7.3, 8.4, 1.6, 2.1, and 1.3 mAh g-1, respectively. -1 After the charge and discharge at different current densities are completed, when the current density returns to 0.1A g -1 When -1 .
[0062] Similarly, in an Ar atmosphere glove box, a CR2016 button cell was assembled with metallic sodium as the counter electrode, NaPF6 / EC:DMC:DEC=1:1:1 (5% FEC) as the electrolyte, and Celgard 2400 membrane as the separator. The electrochemical performance test was then carried out for sodium ion batteries. -1 At the current density, it maintains 330.4 mAh g after 800 cycles. -1 Capacity; at 0.5A g -1 At the current density of 272.9 mAh g, it can maintain 272.9 mAh g after 150 cycles. -1 The capacity of Figure 4 As shown, at 0.1, 0.2, 0.5, 1, 2 and 3A g -1 At current densities of 1.3, 1.7, 1.6, 2.1, 3.2, 1.9, 2.1, and 2.3 mAh g-1, the reversible specific capacities are 397.4, 357.1, 323.6, 292.4, 256.1, and 232.8 mAh g-1, respectively. -1 After the charge and discharge at different current densities are completed, when the current density returns to 0.5 and 0.1 A g -1 When -1 .
[0063] Example 2
[0064] The preparation method and steps of the bismuth / carbon precursor in this embodiment are the same as those in Example 1, but the selenization temperature in the preparation process of the bismuth selenide / carbon composite material is different. Specifically, the Bi / C precursor and selenium powder are ground into uniform powder in a mass ratio of 1:2, placed in a tube furnace, and heated at 3°C min under an argon atmosphere. -1 The temperature was raised at a heating rate of 1.5 °C and selenized and calcined at 600 °C for 2 h. Finally, the black product was collected after cooling to room temperature. The XRD test results are as follows: Figure 1 As shown in Figure 2, XRD test results show that the product is a Bi2Se3 / C composite material. Figure 5 As shown in the transmission electron microscope image, the composite material is a composite structure in which a large number of Bi2Se3 nanodots are embedded in a flaky carbon skeleton, and obvious stacking occurs.
[0065] The composite material is made into a negative electrode sheet and applied to lithium-ion batteries. -1 At the current density, it can maintain 321.3mAh g after 200 cycles. -1 Capacity; at 0.5A g -1 At the current density, it can maintain 348mAh g after 600 cycles. -1 Capacity; at 2A g -1At the current density, it can maintain 224mAh g after 1500 cycles. -1 The capacity of Figure 6 As shown, at 0.1, 0.2, 0.5, 1, 2, 5, 10, 15 and 20A g -1 At current densities of 1.3, 1.7, 2.1, 1.6, 2.3, 3.3, 5.9, 7.3, 8.5 mAh g-1, the reversible specific capacities are 534, 448, 348, 292, 250, 202, 138, 112 and 85 mAh g-1, respectively. -1 After the charge and discharge at different current densities are completed, when the current density returns to 0.1A -1 When -1 .
[0066] Example 3
[0067] The preparation method and steps of the bismuth / carbon precursor in this embodiment are the same as those in Example 1, but the selenization temperature in the preparation process of the bismuth selenide / carbon composite material is different. Specifically, the Bi / C precursor and selenium powder are ground into uniform powder in a mass ratio of 1:2, placed in a tube furnace, and heated at 3°C min under an argon atmosphere. -1 The temperature was raised at a heating rate of 100 °C and selenized and calcined at 900 °C for 2 h. Finally, the black product was collected after cooling to room temperature. The XRD test results are as follows: Figure 1 As shown, the product is a Bi4Se3 / C composite material. Figure 7 As shown in the transmission electron microscopy image, it is a composite structure in which a small amount of Bi4Se3 nanodots are embedded in a flaky carbon skeleton, and the distribution is relatively sparse.
[0068] The composite material was made into a negative electrode sheet and applied to lithium-ion batteries for electrical performance testing. -1 At the current density, it can maintain 390.2mAh g after 200 cycles. -1 Capacity; at 0.5A g -1 At the current density, it can maintain 319mAh g after 600 cycles. -1 Capacity; at 2A g -1 At the current density, it can maintain 162mAh g after 1500 cycles. -1 The capacity of Figure 8 As shown, at 0.1, 0.2, 0.5, 1, 2, 5, 10, 15 and 20A g -1 At current densities of 1.3, 1.7, 2.1, 3.5, 1.6, 1.9, 2.1, 3.5, 1.9, 2.1, 3.5, 1.6, 1.8, 2.1, 3.5, 1.9, 2.1, 3.5 ... -1 ; After the charge and discharge at different current densities are completed, when the current density returns to 0.1A -1 When -1 .
[0069] In summary, the method of the present invention can effectively adjust the Bi:Se atomic ratio in bismuth selenide by regulating the selenization temperature and successfully prepare a new type of Bi x Se y / C composite electrode material, can induce the formation of a stable multi-level structure and interface C-Se bond, effectively improve the structural stability and conductivity of the material, compared with the prior art, the Bi prepared by the present invention x Se y The electrochemical performance of the Bi / C composite material has been significantly improved. x Se y New highs were reached in basic materials.
[0070] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0071] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A Bi x Se y A method for preparing a / C composite material, characterized in that: The following steps are involved: Step S1, directly calcining the organic bismuth salt to obtain a bismuth / carbon precursor material; Step S2: Mix the bismuth / carbon precursor material with selenium and calcine again to obtain Bi x Se y / C composite materials; Where x=3, y=4; In step S1, the calcination temperature is 800-1000°C; In step S2, the calcination temperature is 800°C; In both step S1 and step S2, calcination is performed under an inert atmosphere.
2. Bi according to claim 1 x Se y A method for preparing a / C composite material, characterized in that: The organic bismuth salt is at least one of bismuth citrate, bismuth subsalicylate, bismuth neodecanoate, bismuth subgallate, bismuth isooctanoate, bismuth laurate, and bismuth cyclopentanoate.
3. Bi according to claim 1 x Se y A method for preparing a / C composite material, characterized in that: In step S2, the mass ratio of the bismuth / carbon precursor material to the selenium element is 1:1.5-3.
4. Bi obtained by the preparation method according to any one of claims 1 to 3 x Se y / C composite material.
5. An electrode material, characterized in that: Including the Bi described in claim 4 x Se y / C composite material.
6. A negative electrode, characterized in that Comprising the electrode material according to claim 5.
7. An alkali metal electrochemical energy storage device, characterized in that: Comprising the negative electrode as claimed in claim 6.