A spray film containing nanocellulose and nanosilver, and its preparation method and application
By using L-serine in the spray film spray to synthesize nanosilver and nanocellulose, the problems of poor breathability and high cytotoxicity of traditional nanosilver are solved, and the rapid drying of the spray film spray is achieved and Good antibacterial performance improves patient comfort and the application potential of dressings.
Patent Information
- Application Number
- CN202211526084.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-11-30
AI Technical Summary
The existing film spray film forming materials have poor breathability and strong restraint, which leads to easy tearing and secondary damage to the wound when applied to the wound, reduces the patient's comfort, and the traditional nano-silver synthesis has the problem of high cytotoxicity.
Using L-serine as a carrier to biosynthesize nanosilver under alkaline conditions, and blend it with nanocellulose, polyvinylpyrrolidone, hydroxypropylmethylcellulose, hyaluronic acid, glycerol, propylene glycol and other ingredients to prepare a spray film The agent is used to prepare nanosilver with a number average particle size of 21.27 nm by reacting amino acids with silver nitrate under sodium hydroxide. Combining nanocellulose and other film-forming materials, it forms a transparent film with no irritation and no tension.
The spray spray quickly dry film into films within 10 minutes, with good antibacterial properties and low cytotoxicity, meets the patient's comfort and antibacterial needs, and provides a new type of dermatological medical dressing with potential.
Smart Images

Figure HDA0003973103950000011 
Figure HDA0003973103950000012 
Figure HDA0003973103950000013
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of skin medical dressings, and specifically relates to a spray film containing nanocellulose and nanosilver, a preparation method thereof, and application of the spray film in preparing skin antibacterial medical auxiliary materials. Background Art
[0002] Common medical dressings in clinical practice are mostly in the form of adhesive tapes, gauze, etc., which can easily cause tension mechanical damage, skin maceration and other injuries, and patients have a poor sense of use and reduced compliance. As a new type of skin medical dressing, spray film combines the common advantages of aerosols and film agents, and is easy to use and quick to use. Spray film exists in the form of a solution, and the mixed agent material is dispersed to the skin through an atomizing nozzle. The solvent evaporates in a short time to form a transparent film, which does not affect normal activities and is easy to use. It has good potential for improving the shortcomings of clinical dressings. However, due to some of its limitations, the actual application of spray film agents is still not much, and its biggest limitation is that the film-forming materials of spray film agents are mostly plastic. In the pharmaceutical industry, this feature will produce discomfort characteristics such as poor air permeability and strong sense of restraint. If applied to the wound surface, it is easy to cause secondary damage to the wound surface due to tearing, and the patient's comfort is greatly reduced.
[0003] By consulting the literature, we found that polyvinyl pyrrolidone is a commonly used film-forming material. As a high molecular surfactant, polyvinyl pyrrolidone can be used as a dispersant, emulsifier, thickener, coagulant, cosolvent and detergent in different dispersion systems. It is a high molecular polymer that is easily soluble in polar solvents, has good film-forming properties, has excellent physiological inertness, does not participate in human metabolism, and has excellent biocompatibility, and does not cause any irritation to the skin, mucous membranes, eyes, etc. From a biological point of view, the molecular structure of polyvinyl pyrrolidone is similar to the structure of a simple protein model. Its water solubility, ability to coordinate with certain small molecules, ability to be precipitated by certain protein precipitants, and compatibility with proteins make polyvinyl pyrrolidone widely used as an excipient for pharmaceutical preparations.
[0004] Polyvinyl pyrrolidone is not tough enough when used alone, so it can be used in combination with materials with strong mechanical properties. Hydroxypropyl methylcellulose is a kind of material with strong mechanical properties. Hydroxypropyl methylcellulose has good film-forming properties, high safety, and good sustained-release effect. It has become the most widely used film coating material in China. When used alone in spray film, the viscosity is slightly higher, so the general concentration should not be too high. It is often used in combination with other film-forming materials in film applications. Nanocellulose is a kind of renewable, high aspect ratio nanoparticles with high mechanical properties and a cross-section of 5-20nm and a length of 10nm-1um. Due to the characteristics of nanoparticles, nanocellulose has the characteristics of high crystallinity, high specific surface area, high modulus, strong hydrophilicity and high surface activity. At the same time, it has the advantages of light weight, degradability, biocompatibility and renewability of biomaterials, highlighting good mechanical properties and hydrophilic properties, which can significantly improve the comprehensive performance of polymers, and can also open up new ideas and ways for the efficient use of biomass resources. It is considered to be a green reinforcement material with great development potential.
[0005] In order to increase the comfort of patients, the spray film material should also have basic skin water retention. Hyaluronic acid, glycerin, propylene glycol, etc. are several commonly used materials for skin moisturizing. Hyaluronic acid is an acidic mucopolysaccharide and a biochemical drug with high clinical value. It can play a unique role in protecting the skin when used in skin preparations. It can keep the skin moisturized, smooth, delicate, tender and elastic. It has the functions of anti-wrinkle, anti-wrinkle, beauty care and restoration of skin physiological functions. Glycerin is a natural oil extracted from the seeds of olive plants. It has many functions such as sun protection, moisturizing, reducing wrinkles and preventing chapped lips. Propylene glycol is often used as a wetting agent in cosmetics, toothpaste and soap in combination with glycerin or sorbitol, and is also used as an antifreeze agent. Glycerin and propylene glycol are both polyol compounds, which can be used as plasticizers, surfactants, emulsifiers and demulsifiers. Polyol compounds have multiple hydroxyl groups in their chemical structure and can play a good moisturizing role. Therefore, glycerin and propylene glycol are often used as moisturizers.
[0006] The spray film should also have good antibacterial properties. It has long been known that the surface of large silver materials has antibacterial properties. The mechanism is that the silver atoms on the surface of the material can be slowly oxidized by oxygen in the environment to release free silver ions. These silver ions bind to the thiol groups on the bacterial wall, blocking the respiratory chain of the bacteria and eventually killing the bacteria attached to the surface of the material. Nanosilver reacts faster than large silver and has greater advantages. Silver nitrate is often used as a raw material for synthesizing nanosilver. L-serine is one of the essential amino acids for the human body and is a non-essential amino acid. It is more economical and easy to obtain than other amino acids. As a basic amino acid that constitutes protein, it is widely used in medicine, food, cosmetics and other industries. It is an important precursor for the synthesis of intracellular biological substances such as purine, pyrimidine, and phospholipids. In addition, because L-serine has special wettability and moisturizing properties, it is widely used in advanced cosmetics at home and abroad. We designed to use L-serine as a carrier to biosynthesize nanosilver, and use the uptake of L-serine by bacteria to achieve good antibacterial effects.
[0007] The invention firstly prepares nano silver with a number average particle size of 21.27 nm by biosynthesis of BOC-L-serine and silver nitrate under alkaline conditions (sodium hydroxide). The nano silver has a cell survival rate of more than 80% compared with normal cells within a concentration range of 300 μg / ml, and has less damage to cells. Conventional synthesized nano silver has strong cytotoxicity between 50 and 125 μg / ml, resulting in a low cell survival rate. The nano silver synthesized by the invention has lower cytotoxicity and higher cell survival rate. The nano silver has a minimum inhibitory concentration of 25 μg / ml and a minimum bactericidal concentration of 50 μg / ml for common clinical strains (methicillin-sensitive Staphylococcus aureus, carbapenem-sensitive Escherichia coli, methicillin-resistant Staphylococcus aureus and carbapenem-resistant Escherichia coli), and has a greater antibacterial advantage than conventional chemically synthesized nano silver (minimum inhibitory concentration ≥100 μg / ml, minimum bactericidal concentration ≥500 μg / ml).
[0008] On this basis, the nanosilver is mixed with nanocellulose, polyvinyl pyrrolidone, hydroxypropyl methylcellulose, hyaluronic acid, glycerol, propylene glycol, deionized water and ethanol to prepare a spray film. The spray film can be quickly dried into a film within 10 minutes. After drying, it is colorless and transparent. The film itself is non-irritating and has no obvious tightness. It does not affect the normal activity of the skin. The drug can be directly administered again on the newly formed film. It has the advantages of easy use and good feel. The addition of nanosilver makes the spray film have good antibacterial advantages, which greatly meets the various needs of patients. It is a new type of skin medical dressing with good potential. Summary of the invention
[0009] The purpose of the present invention is to provide a spray film containing nanocellulose and nanosilver and a preparation method and application thereof. The spray film of the present invention has good biocompatibility and good antibacterial effect.
[0010] In order to achieve the above object, the present invention adopts the following technical scheme:
[0011] In a first aspect, the present invention provides a spray containing nanocellulose and nanosilver, wherein the spray containing nanocellulose and nanosilver is substantially composed of the following components in mass concentrations: 0.01% to 16.6% polyvinyl pyrrolidone, 0.001% to 0.8% hydroxypropyl methylcellulose, 0.001% to 0.8% sodium hyaluronate, 0.1% to 3.33% glycerol, 0.1% to 3.33% propylene glycol, 0.01% to 0.67% nanocellulose, 0.001% to 0.02% nanosilver, and the solvent is water or a mixed solvent of water and ethanol;
[0012] The nano silver is prepared as follows:
[0013] An amino acid or an amino acid derivative and silver nitrate are dissolved in deionized water, and an aqueous solution of an alkaline substance is added dropwise. After the addition is completed, the resulting mixed solution is reacted at room temperature for 5-12 hours (6 hours in one embodiment of the present invention), and the resulting reaction solution is post-treated to obtain the nanosilver; the amino acid derivative is an amino acid whose amino group is protected by a protecting group, and the amount ratio of the amino acid or amino acid derivative, silver nitrate and the alkaline substance in the aqueous solution of the alkaline substance is 1:1-5:1.5-2.5 (preferably 1:1-2:2, most preferably 1:1:2); the alkaline substance in the aqueous solution of the alkaline substance is sodium hydroxide or potassium hydroxide.
[0014] "Substantially" means that the above components are the main components of the spray film, and other components may be appropriately added. The other components are excipients acceptable to the human body.
[0015] Furthermore, the spray film containing nanocellulose and nanosilver may also include auxiliary materials acceptable to human body with a mass concentration of less than 3.3%.
[0016] Furthermore, the auxiliary material is one or more of tea tree essential oil, propolis, and polyvinyl alcohol. The inventor has added 3.3% essential oil, 0.46% propolis, or 3.3% polyvinyl alcohol, and the spray morphology of the obtained spray film agent remains basically unchanged.
[0017] The embodiment of the present invention provides a basic formula, but those skilled in the art should know that the addition of other compatible excipients acceptable to the human body is also within the scope of the present invention. The basic formula is: the spray film containing nanocellulose and nanosilver is composed of the following components in mass concentration: polyvinyl pyrrolidone 0.01% to 16.6%, hydroxypropyl methylcellulose 0.001% to 0.8%, sodium hyaluronate 0.001% to 0.8%, glycerol 0.1% to 3.33%, propylene glycol 0.1% to 3.33%, nanocellulose 0.01% to 0.67%, nanosilver 0.001% to 0.02%, and the solvent is water or a mixed solvent of water and ethanol.
[0018] The present invention particularly recommends that the spray containing nanocellulose and nanosilver is basically composed of the following components in mass concentration: 3.33% polyvinyl pyrrolidone, 0.047% hydroxypropyl methylcellulose, 0.17% sodium hyaluronate, 1.67% glycerol, 1.67% propylene glycol, 0.53% nanocellulose, and the solvent is water or a mixed solvent of water and ethanol; the amount of nanosilver can be selected according to needs. In one embodiment of the present invention, the mass concentration of the nanosilver is 0.008%-0.013%.
[0019] In one embodiment of the present invention, the polyvinyl pyrrolidone is K30. The hydroxypropyl methylcellulose is E30. The sodium hyaluronate is an oligomeric sodium hyaluronate having a molecular weight of less than 10 kDa. The diameter of the nanocellulose is 500 to 1000 μm and the length is 20-100 μm. The above polymers are all common raw materials in the art. The above specific types should not be understood as limitations of the present invention, and replacement of polymers with other molecular weights should also be within the scope of protection of the present invention. For example, the role of nanocellulose is to reduce the fluidity of the spray, and nanocellulose of other sizes can also achieve the purpose of the present invention.
[0020] The invention prepares nanosilver with a number average particle size of 21.27 nm by biosynthesis of amino acids and silver nitrate under alkaline conditions (sodium hydroxide). The nanosilver has a cell survival rate of more than 80% compared with normal cells within a concentration range of 300 μg / ml, and causes less damage to cells. Conventional synthesized nanosilver shows strong cytotoxicity at a concentration between 50 and 125 μg / ml, resulting in a low cell survival rate. In comparison, the nanosilver synthesized by the invention has lower cytotoxicity and higher cell survival rate, and the nanosilver has a greater antibacterial advantage against common clinical strains.
[0021] The material mixing order and ratio of the nanosilver synthesis described in the present invention are demanding, and the alkaline substance must be added last in the preparation process. When the amount of silver nitrate used is less than the range of the present invention, it is difficult to obtain nanosilver; when the amount of silver nitrate used is greater than the range of the present invention, the conversion rate is low, which will cause waste of silver nitrate. When the amount of sodium hydroxide used is too high, it will generate silver hydroxide precipitate with silver nitrate; when the amount of sodium hydroxide used is too low, it cannot fully activate amino acids.
[0022] Preferably, when an amino acid whose amino group is protected by a protecting group participates in the reaction, the yield of nanosilver is higher, for example, the protecting group is a Boc group, a Trt group or a Fmoc group. In one embodiment of the present invention, the amino acid is serine, and the amino acid derivative is serine protected by Boc.
[0023] Furthermore, in the mixed solution, the concentration of silver nitrate is 10-100 mM (50 mM in one embodiment of the present invention).
[0024] In the embodiment of the present invention, silver nitrate, amino acid and alkaline substance are first configured into aqueous solution and then mixed in order to disperse them evenly, reduce the number of weighing times and facilitate the experiment.
[0025] Furthermore, the post-treatment is as follows: the reaction solution is centrifuged (15000 rpm for 15 min), the obtained precipitate is washed with deionized water (3 times), and freeze-dried to obtain the nanosilver.
[0026] Furthermore, in one embodiment of the present invention, when the solvent is a mixed solvent of water and ethanol, the mass of water is 26.6% to 99.7% of the spray agent containing nanocellulose and nanosilver.
[0027] In a second aspect, the present invention provides a method for preparing the above-mentioned spray agent containing nanocellulose and nanosilver, the method comprising the following steps: fully dispersing the composition amounts of polyvinyl pyrrolidone, hydroxypropyl methylcellulose, sodium hyaluronate, glycerol, propylene glycol, nanocellulose, and nanosilver in a solvent to obtain the spray agent containing nanocellulose and nanosilver.
[0028] In one embodiment of the present invention, in order to disperse evenly, the dispersion is carried out as follows: polyvinyl pyrrolidone and hydroxypropyl methylcellulose are dissolved in a solvent, sodium hyaluronate, glycerol, propylene glycol, and a 2% by mass nanocellulose aqueous solution are added, and dispersed evenly, nanosilver is added, and dispersed evenly to obtain the nanocellulose and nanosilver spray agent.
[0029] In a third aspect, the present invention provides a use of the above-mentioned spray film containing nanocellulose and nanosilver as a skin medical dressing.
[0030] Compared with the prior art, the beneficial effects of the present invention are as follows: the film spraying agent of the present invention can be quickly dried to form a film within 10 minutes, and is colorless and transparent after drying. The film itself is non-irritating and has no obvious tightness, and does not affect the normal activity of the skin. The drug can be directly administered again on the newly formed film, and it has the advantages of being easy to use and having a good feel of use. Nanosilver can destroy bacteria and rupture bacterial cells to achieve an antibacterial effect, providing the film spraying agent with good antibacterial properties, which can greatly meet the various needs of patients. It is a new type of skin medical dressing with good potential and is expected to be widely used in the fields of life sciences and medicine. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 :Energy spectrum scanning of nano silver powder
[0032] Figure 2 :Dynamic light scattering nanoparticle size analyzer detection image of nano silver powder
[0033] Figure 3 :Cell survival rate at different nanosilver concentrations
[0034] Figure 4 :Minimum inhibitory concentration and minimum bactericidal concentration of nanosilver against methicillin-sensitive Staphylococcus aureus, carbapenem-sensitive Escherichia coli, methicillin-resistant Staphylococcus aureus and carbapenem-resistant Escherichia coli DETAILED DESCRIPTION
[0035] The present invention is further described in conjunction with the accompanying drawings and embodiments.
[0036] In the following examples, the polyvinyl pyrrolidone is K30.
[0037] Example 1 Biosynthesis of Nanosilver from BOC-L-serine
[0038] Slowly drop 1 ml of 0.5 M sodium hydroxide solution into a mixed solution of 2.5 ml of 0.1 M BOC-L serine and 1 ml of 0.5 M silver nitrate, and dilute to 10 ml with deionized water. React at room temperature for 6 h, centrifuge at 15000 rpm for 15 min, discard the supernatant and wash with deionized water, wash with deionized water 3 times, freeze-dry, and obtain nano silver powder. The conversion rate of nano silver was determined to be 84.5%. The main components of the obtained product were detected by energy spectrum scanner, such as Figure 1 As shown in the energy spectrum scanning diagram, the powder has a sharp and obvious peak at the absorption peak of silver element, which can determine that the main component of the powder is silver element; the number average particle size of the nanosilver is measured by a dynamic light scattering nanoparticle size analyzer, as shown in FIG. Figure 2As shown, it can be seen that the number average particle size of the nanosilver is 21.27nm; methicillin-sensitive Staphylococcus aureus, carbapenem-sensitive Escherichia coli, methicillin-resistant Staphylococcus aureus and carbapenem-resistant Escherichia coli are used as model strains, and the minimum inhibitory concentration and minimum bactericidal concentration of nanosilver for the model strains are determined by the microbroth dilution method, 180μL of broth culture fluid is added to all wells of the 96-well plate, and then 100μL of broth culture fluid is added to each well, 20μL of drug solution is added to all wells in the first column, and no drug solution is added to the first well of the last row; the solution in the first well of each row is blown evenly, and then 100μL of solution is taken out and added to the next well in the same row, the pipette blows several times to mix the solution evenly, and then 100μL of solution is aspirated and moved to the next well in the same row, and diluted to the last well according to this method, and 100μL of solution is aspirated and discarded after the last well is mixed evenly; the last row is set as a blank control group without any antibacterial drug. Add 10 μL of the diluted solution to a concentration of 10 to the first nine wells of the last row. 5 CFU / ml of bacterial solution; and 10μL of broth culture solution is added to the last well. Transfer the well plate to a biochemical incubator, set the temperature to 37°C, and culture for 16-20 hours. In order to keep the culture temperature of the solution in each experimental group the same, no more than 4 96-well plates should be placed overlapping. The solution in each well can be distinguished by the naked eye as clear or turbid. The clarity of the solution observed by the naked eye indicates that the drug solution can completely inhibit bacterial growth. Therefore, the minimum drug concentration corresponding to the clear and transparent solution in the well without suspension is the minimum inhibitory concentration of the drug sample for the corresponding strain. Take 10μL from the front and back 3 wells corresponding to the minimum inhibitory concentration and spread it on the agar plate. After culturing at 37°C for 16-20 hours, the concentration corresponding to no colony growth or only single colony growth is the minimum bactericidal concentration. The three groups were measured in parallel. The results are as follows Figure 4 As shown in the figure, the minimum inhibitory concentration of the nanosilver against common clinical strains (methicillin-sensitive Staphylococcus aureus, carbapenem-sensitive Escherichia coli, methicillin-resistant Staphylococcus aureus and carbapenem-resistant Escherichia coli) is 25μg / ml, and the minimum bactericidal concentration is 50μg / ml; using normal human immortalized keratinocytes as a cell model, the cell survival rate of the nanosilver was detected at 630nm and 450nm wavelengths by combining CCK-8 detection method with dual wavelength method, and the results are as follows Figure 3 As shown, within the concentration range of 300 μg / ml, the cell survival rate can reach 80% of normal cells.
[0039] Example 2 Biosynthesis of Nanosilver from L-Serine
[0040] Slowly drop 1 ml of 0.5 M sodium hydroxide solution into a mixed solution of 2.5 ml of 0.1 M L amino acid and 1 ml of 0.5 M silver nitrate, and dilute to 10 ml with deionized water. React at room temperature for 5-12 hours, centrifuge at 15000 rpm for 15 minutes, discard the supernatant and wash with deionized water, wash with deionized water 3 times, freeze-dry, and obtain nanosilver powder. The conversion rate of nanosilver is 84.5% after measurement.
[0041] Example 3 Preparation of Nano-Spray Film Based on Nanocellulose
[0042] 1 g of polyvinyl pyrrolidone (K30) and 0.014 g of hydroxypropyl methylcellulose (E30) were accurately weighed and dissolved in deionized water, and 0.05 g of sodium hyaluronate (Huaxi Freda Biopharmaceutical Co., Ltd., batch number: 1711093), 0.5 g of glycerol, and 0.5 g of propylene glycol were added. After fully dissolved, 8 g of a 2% aqueous solution of nanocellulose (Guilin Qihong Technology Co., Ltd., diameter 500-1000 μm, length 20-100 μm) was added, and deionized water was added to make the total mass 30 g. 2.4 mg of the nanosilver in Example 1 was added and dissolved to obtain a nano-spray agent containing nanocellulose.
[0043] Example 4 Preparation of Nano-cellulose-based Nano-spray Film
[0044] 1 g of polyvinyl pyrrolidone (K30) and 0.014 g of hydroxypropyl methylcellulose (E30) were accurately weighed and dissolved in deionized water, and 0.05 g of sodium hyaluronate (Huaxi Freda Biopharmaceutical Co., Ltd., batch number: 1711093), 0.5 g of glycerol, and 0.5 g of propylene glycol were added. After fully dissolved, 10 g of a 2% nanocellulose solution (Guilin Qihong Technology Co., Ltd., diameter 500-1000 μm, length 20-100 μm) was added, and deionized water was added to make the total mass 30 g. 3 mg of the nanosilver in Example 1 was added and dissolved to obtain a nano-spray agent containing nanocellulose.
[0045] Example 5 Preparation of Nano-Spray Film Based on Nanocellulose
[0046] 1 g of polyvinyl pyrrolidone (K30) and 0.014 g of hydroxypropyl methylcellulose (E30) were accurately weighed and dissolved in deionized water, and 0.05 g of sodium hyaluronate (Huaxi Freda Biopharmaceutical Co., Ltd., batch number: 1711093), 0.5 g of glycerol, and 0.5 g of propylene glycol were added. After fully dissolved, 6 g of a 2% nanocellulose solution (Guilin Qihong Technology Co., Ltd., diameter 500-1000 μm, length 20-100 μm) was added, and deionized water was added to make the total mass 30 g. 4 mg of the nanosilver in Example 1 was added and dissolved to obtain a nano-spray agent containing nanocellulose.
[0047] Example 6 Preparation of Nano-cellulose-based Nano-spray Film
[0048] 1 g of polyvinyl pyrrolidone (K30) and 0.05 g of hydroxypropyl methylcellulose (E30) were accurately weighed and dissolved in deionized water, 0.15 g of sodium hyaluronate (Huaxi Freda Biopharmaceutical Co., Ltd., batch number: 1711093), 1 g of glycerol, and 1 g of propylene glycol were added, and after fully dissolved, 6 g of a 2% nanocellulose solution (Guilin Qihong Technology Co., Ltd., diameter 500-1000 μm, length 20-100 μm) was added, 15 g of deionized water and 5.8 g of ethanol were added to make the total mass 30 g, and 3 mg of the nanosilver in Example 1 was added to dissolve to obtain a nano-spray agent containing nanocellulose.
[0049] Example 7 Preparation of Nano-cellulose-based Nano-spray Film
[0050] 1.5 g of polyvinyl pyrrolidone (K30) and 0.08 g of hydroxypropyl methylcellulose (E30) were accurately weighed and dissolved in deionized water, and 0.08 g of sodium hyaluronate (Huaxi Freda Biopharmaceutical Co., Ltd., batch number: 1711093), 0.8 g of glycerol, and 0.8 g of propylene glycol were added. After fully dissolved, 10 g of a 2% nanocellulose solution (Guilin Qihong Technology Co., Ltd., diameter 500-1000 μm, length 20-100 μm) was added, and deionized water was added to make the total mass 30 g. 3 mg of the nanosilver in Example 1 was added and dissolved to obtain a nano-spray agent containing nanocellulose.
[0051] In each group of formulas of Examples 3 to 7, the spray film was sprayed on the skin and its fluidity was measured by the atomization condition (the state was distinguished by columnar, branched, and water mist, and the water mist was the best state). Among them, Examples 3, 5, and 6 were all well atomized, while Examples 4 and 7 were sprayed in a columnar shape and the atomization condition was not good. However, the strong fluidity of the spray film in Examples 5 and 6 was not conducive to being retained on the skin. Therefore, the ratio of Example 3 was the best condition. Therefore, the best ratio of each component of the spray film was determined to be: 1g of polyethylene Pyrrolidone, 0.014g hydroxypropyl methylcellulose, 0.05g sodium hyaluronate, 0.5g glycerol, 0.5g propylene glycol, 8g of 2% nanocellulose aqueous solution (Guilin Qihong Technology Co., Ltd., MFC) were added; the spray film prepared in Example 3 was placed in a 4°C refrigerator, room temperature, and a 37°C oven for 48h, and the stratification phenomenon of the spray film at different temperatures was observed to determine the stability of the spray film (if stratification occurs, it is unstable, and no stratification indicates a stable state). It was determined that the spray film under this formula had no obvious stratification phenomenon.
Claims
1. A spray film containing nanocellulose and nanosilver, characterized in that The spray containing nanocellulose and nanosilver is basically composed of the following components in mass concentrations: 0.01% to 16.6% polyvinyl pyrrolidone, 0.001% to 0.8% hydroxypropyl methylcellulose, 0.001% to 0.8% sodium hyaluronate, 0.1% to 3.33% glycerol, 0.1% to 3.33% propylene glycol, 0.01% to 0.67% nanocellulose, 0.001% to 0.02% nanosilver, and the solvent is water or a mixed solvent of water and ethanol; The nano silver is prepared as follows: The amino acid or amino acid derivative and silver nitrate are dissolved in deionized water, and an aqueous solution of an alkaline substance is added dropwise. After the addition is completed, the obtained mixed solution is reacted at room temperature for 5-12 hours, and the obtained reaction solution is post-treated to obtain the nanosilver; the post-treatment is centrifuging the reaction solution, washing the obtained precipitate with deionized water, and freeze-drying. The amino acid derivative is an amino acid whose amino group is protected by a protecting group, and the amount ratio of the amino acid or amino acid derivative, silver nitrate and the alkaline substance in the aqueous solution of the alkaline substance is 1:1-5:1.5-2.5; the alkaline substance in the aqueous solution of the alkaline substance is sodium hydroxide or potassium hydroxide; the amino acid is serine, and the amino acid derivative is serine protected by Boc.
2. The spray film containing nanocellulose and nanosilver as claimed in claim 1, characterized in that: The spray film containing nanocellulose and nanosilver also includes auxiliary materials acceptable to human body with a mass concentration of less than 3.3%.
3. The spray film containing nanocellulose and nanosilver as claimed in claim 2, characterized in that: The auxiliary materials are one or more than two of tea tree essential oil, propolis and polyvinyl alcohol.
4. The spray film containing nanocellulose and nanosilver as claimed in claim 1, characterized in that The spray containing nanocellulose and nanosilver is composed of the following components in mass concentrations: 0.01% to 16.6% polyvinyl pyrrolidone, 0.001% to 0.8% hydroxypropyl methylcellulose, 0.001% to 0.8% sodium hyaluronate, 0.1% to 3.33% glycerol, 0.1% to 3.33% propylene glycol, 0.01% to 0.67% nanocellulose, and 0.001% to 0.02% nanosilver, and the solvent is water or a mixed solvent of water and ethanol.
5. The spray film containing nanocellulose and nanosilver as claimed in claim 1, characterized in that The spray containing nanocellulose and nanosilver is basically composed of the following components in mass concentration: 3.33% polyvinyl pyrrolidone, 0.047% hydroxypropyl methylcellulose, 0.17% sodium hyaluronate, 1.67% glycerol, 1.67% propylene glycol, 0.53% nanocellulose, the mass concentration of nanosilver is 0.008%-0.013%, and the solvent is water or a mixed solvent of water and ethanol.
6. The spray film containing nanocellulose and nanosilver as claimed in claim 1, characterized in that: The amino acid is an amino acid whose amino group is protected by a protecting group, and the protecting group is a Boc group, a Trt group or a Fmoc group.
7. The spray film containing nanocellulose and nanosilver as claimed in claim 1, characterized in that: In the mixed solution, the concentration of silver nitrate is 10-100 mM.
8. The spray film containing nanocellulose and nanosilver as claimed in claim 1, characterized in that: The post-treatment is as follows: the reaction solution is centrifuged, the obtained precipitate is washed with deionized water, and freeze-dried to obtain the nano-silver.
9. The method for preparing the spray film containing nanocellulose and nanosilver as claimed in claim 1, characterized in that The method comprises the following steps: fully dispersing the composition amount of polyvinyl pyrrolidone, hydroxypropyl methylcellulose, sodium hyaluronate, glycerol, propylene glycol, nanocellulose and nanosilver in a solvent to obtain the spray film containing nanocellulose and nanosilver.
10. Use of the spray film containing nanocellulose and nanosilver as claimed in claim 1 in preparing a skin medical dressing.