Method for preparing 3D network interpenetrating molybdenum disulfide thin film using self-excited non-zero oscillation high power pulse technology
Through vacuum self-excitation non-zero position oscillation high-power micro-pulse magnetron sputtering technology, the density and tribological properties of the interpenetrating molybdenum disulfide film of 3D network are improved, and the problem of low target ionization rate in the existing technology is solved. , achieving higher friction life and wear resistance.
Patent Information
- Application Number
- CN202211558856.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-06
AI Technical Summary
When the existing magnetron sputtering technology prepares 3D network interpenetrating molybdenum disulfide films, the ionization rate of the target is generally low, resulting in insufficient film-forming density and tribological performance, which makes it difficult to meet the needs of complex service environments.
Using vacuum self-excitation non-zero oscillation high-power micro-pulse magnetron sputtering technology, the ionization rate of the target is significantly improved by adjusting the chamber pressure, bias voltage and pulse parameters, and the ionization rate of the target is significantly improved, and the TiN transition layer and 3D network interpenetrating disulfide are deposited. Molybdenum films inhibit unidirectional growth mode and enhance the density and binding force of the film.
It significantly improves the density and tribological properties of the 3D network interpenetrating molybdenum disulfide film, improves the film's load-bearing capacity and wear resistance, extends the friction life, and shows excellent tribological properties especially in vacuum environments.
Smart Images

Figure CN115786848B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing a molybdenum disulfide film by using a magnetron sputtering technology, and in particular to a method for preparing a 3D network interpenetrating molybdenum disulfide film by using a vacuum self-excited non-zero position oscillation high-power micro-pulse magnetron sputtering technology, belonging to the field of vacuum coating technology and the field of tribology. Background Art
[0002] 3D network interpenetrating molybdenum disulfide is a transition metal chalcogenide. The atoms in its layers are tightly bound together by S-Mo-S covalent bonds, and the interlayers are bound by weak van der Waals forces. It is this unique layered structure that gives it good lubrication ability (especially under vacuum conditions) and is often used as a lubricating material in the industrial field. Preparing anti-friction and anti-wear coatings in the form of 3D network interpenetrating molybdenum disulfide films is a stable and reliable method that can give full play to its high load-bearing performance to meet complex service environments.
[0003] Among the current methods for preparing 3D network interpenetrating molybdenum disulfide films, magnetron sputtering is widely used as a method that can obtain high film density, high film uniformity, and good film-base bonding. Currently, the commonly used magnetron sputtering technologies mainly include medium-frequency magnetron sputtering, radio frequency magnetron sputtering, and reactive magnetron sputtering, but the ionization rate of the target material in these methods is generally low, so there is still room for improvement in the density of the film. Compared with other magnetron sputtering processes, the method of self-excited non-zero-position oscillation high-power micro-pulse magnetron sputtering can significantly improve the ionization rate of the target material, which is of great help in preparing a denser and more uniform 3D network interpenetrating molybdenum disulfide film to reduce its film defects, so as to further improve its tribological properties, and has important application value. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a 3D network interpenetrating molybdenum disulfide film by using self-excited non-zero oscillation high-power micro-pulse magnetron sputtering technology, so as to improve the ionization rate of the target material and the tribological properties of the film.
[0005] 1. Preparation of 3D network interpenetrating MoS2 thin films
[0006] The method for preparing a 3D network interpenetrating molybdenum disulfide film of the present invention is to deposit a 3D network interpenetrating molybdenum disulfide film on the surface of a substrate by using a vacuum self-excited non-zero position oscillation high-power micro-pulse magnetron sputtering technology. The specific deposition process is as follows:
[0007] (1) The substrate was ultrasonically cleaned with acetone and alcohol for 20-30 min to remove surface impurities and organic matter; it was blown dry with nitrogen and placed on the sample holder of the magnetron sputtering chamber, and the chamber was evacuated to a pressure of less than 1×10 -3Pa; then introduce high-purity argon gas, adjust the argon gas flow rate to make the chamber pressure reach 2.0~3.0Pa, adjust the bias voltage to -700~-800V, and perform bias cleaning on the substrate surface to remove impurities on the substrate surface. The substrate is a stainless steel sheet or a single crystal silicon sheet;
[0008] (2) High-purity nitrogen was introduced, and the flow ratio of argon and nitrogen was controlled to be 10:1; the chamber pressure was adjusted to 1.0~1.3Pa, the bias voltage was adjusted to -50~-100V, and the TiN transition layer was deposited by magnetron sputtering Ti target: the average current of Ti target was 0.85A, and the target voltage was 600V; the duty cycle of self-excited non-zero oscillation high-power micro-pulse magnetron sputtering power supply was 10%, and the pulse length was 125us; the deposition time was 20~25min, and the deposition thickness of TiN transition layer was 150~200nm;
[0009] (3) Turn off and stop the nitrogen flow, adjust the chamber pressure to 1.0~1.3Pa, adjust the bias voltage to -50~-80V, and magnetron sputter 3D network interpenetrating MoS2 target to deposit 3D network interpenetrating MoS2 film; the average current of 3D network interpenetrating MoS2 target is 0.39~0.42A, and the target voltage is 650V; the duty cycle of self-excited non-zero oscillation high-power micro-pulse magnetron sputtering power supply is 10%, and the pulse length is 83~125us; the deposition time is 120min, and the deposition thickness of 3D network interpenetrating MoS2 film is 2.2~3.1um.
[0010] Figure 1 The target current and target voltage data recorded by the oscilloscope during the deposition process. Among them, (a) is the target current and target voltage data under a pulse width of 125us; (b) is the target current and target voltage data under a pulse width of 83us. In the process of self-excited non-zero oscillation high-power micro-pulse magnetron sputtering, the pulse discharge stage can provide a larger peak power, which provides a larger particle energy to the target particles. The target particles have greater kinetic energy when deposited on the substrate, and the generated particle bombardment effect is greater, which is more capable of inhibiting MoS 2 The unidirectional growth mode during the deposition process reduces the nucleation radius and increases the nucleation sites, making the growing MoS 2 The film is denser.
[0011] The schematic diagram of the structure of the 3D network interpenetrating molybdenum disulfide film obtained by the present invention is as follows Figure 2 As shown in the figure, the TiN transition layer and the substrate have a smaller lattice mismatch, which reduces the interlayer stress during the film deposition process, so that the substrate and the 3D network interpenetrating molybdenum disulfide film have good bonding strength; and TiN itself is a material with high hardness, and deposition as a transition layer can improve the load-bearing capacity of the film.
[0012] Figure 3The SEM images of the 3D network interpenetrating molybdenum disulfide film prepared by the present invention. (a) and (b) are the cross-sectional and surface SEM images of the molybdenum disulfide film deposited by the self-excited non-zero oscillation high-power micro-pulse magnetron sputtering technology; (c) and (d) are the cross-sectional and surface SEM images of the 3D network interpenetrating molybdenum disulfide film deposited by the medium-frequency magnetron sputtering technology. Figure 3 It can be seen that the thickness of the TiN transition layer is 160nm, and the thickness of the 3D network interpenetrating MoS2 film is 2.2um. The cross section of the 3D network interpenetrating MoS2 film is dense, without obvious columnar growth; the interface between the TiN transition layer and the 3D network interpenetrating MoS2 film is not obvious, indicating that they are well combined; the surface of the 3D network interpenetrating MoS2 film is flat and dense, without obvious defects.
[0013] Figure 4 HRTEM images of the 3D network interpenetrating MoS2 thin film prepared by the present invention. (a) is a 3D network interpenetrating MoS2 thin film deposited by medium frequency magnetron sputtering technology at high magnification; (b) is a 3D network interpenetrating MoS2 thin film deposited by self-excited non-zero position oscillation high power micropulse technology at high magnification. Figure 4 It can be seen from the figure that the 3D network interpenetrating molybdenum disulfide film prepared by the present invention is a short-range ordered nanocrystalline structure with refined grains and obvious curvature of the crystal plane. The measured interlayer spacing is 0.67nm. The structure of the TiN transition layer is obviously different from that of the molybdenum disulfide film. TiN has a smaller intercrystalline spacing, which indicates that the process suppresses the traditional MoS 2 The unidirectional columnar growth mode during the film deposition process improves the organizational density of the film, thereby improving the mechanical properties of the film, which is significantly different from the medium-frequency magnetron sputtering deposition film.
[0014] 2. Performance of 3D Network Interpenetrating MoS2 Films
[0015] Using Anton Paar NHT 2 The nanoindenter measures the microhardness and elastic modulus of the film by continuous indentation. The maximum indentation depth is set to 150nm (to ensure that the indentation depth of the indenter is less than 1 / 10 of the film thickness during the test to avoid the influence of the substrate on the hardness test); at the same time, in order to reduce the measurement error, 5 points are selected for each sample during the test, and the average value is used as the final result of the experiment. The hardness of the 3D network interpenetrating molybdenum disulfide film is measured between 2.76 and 3.55GPa, and the elastic modulus is between 48.59 and 62.65GPa.
[0016] The friction and wear properties of 3D network interpenetrating molybdenum disulfide film in vacuum and atmospheric environment were measured by ball-disc friction machine. The selected friction load was 10N, the rotation speed was 200rpm, the friction pair was Φ3mm 440c stainless steel ball, the friction radius was 3mm, and the friction coefficient was greater than 0.2, which was considered as film failure. Under vacuum friction conditions, the ambient pressure was less than 5×10 -3 Pa, and the ambient humidity in the atmospheric environment was controlled between 20 and 25% RH. In addition, the friction life of the 3D network interpenetrating molybdenum disulfide film under the two environments was tested respectively; the wear volume of the wear scar was obtained after the friction test using the Micro XAM non-contact three-dimensional surface profiler, and the wear rate was calculated using the formula K=V / FS, where K is the wear rate, V is the wear volume, F is the friction load, and S is the total stroke.
[0017] Through the above friction test parameters, the friction coefficient of 3D network interpenetrating MoS2 film in vacuum environment is stable between 0.035 and 0.045; the calculated wear rate is 8.61×10 -8 mm -3 / Nm~9.24×10 -8 mm -3 The friction coefficient in the atmospheric environment is stable between 0.06 and 0.08, the friction life is not less than 100,000 cycles, and the calculated wear rate is 6.05×10 -7 mm -3 / Nm~7.37×10 -7 mm -3 The friction life measured in vacuum environment is greater than 900,000 cycles, and the friction life measured in atmospheric environment is greater than 100,000 cycles (see Figure 5 ).
[0018] In summary, the 3D network interpenetrating molybdenum disulfide film prepared by vacuum self-excited non-zero-position oscillation high-power micropulse magnetron sputtering in the present invention has good bonding force with the substrate, and the obtained 3D network interpenetrating molybdenum disulfide film has high density and low defects, which effectively improves the load-bearing capacity and wear resistance of the 3D network interpenetrating molybdenum disulfide film, increases the friction life of the film, and has excellent tribological properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The target current and target voltage data are recorded by an oscilloscope during the preparation of the 3D network interpenetrating molybdenum disulfide film of the present invention.
[0020] Figure 2 This is a schematic diagram of the structure of the 3D network interpenetrating molybdenum disulfide film prepared by the present invention.
[0021] Figure 3This is a SEM image of the 3D network interpenetrating molybdenum disulfide film prepared in the present invention.
[0022] Figure 4 This is the HRTEM image of the 3D network interpenetrating molybdenum disulfide film prepared in the present invention.
[0023] Figure 5 This is a friction life diagram of the 3D network interpenetrating molybdenum disulfide film prepared by the present invention. DETAILED DESCRIPTION
[0024] The following is a further description of the method and performance of preparing a 3D network interpenetrating molybdenum disulfide thin film using magnetron sputtering technology according to the present invention through specific examples.
[0025] Example 1
[0026] (1) The substrate was ultrasonically cleaned with acetone and alcohol for 20-30 min to remove surface impurities and organic matter, then dried with nitrogen and placed on the sample holder of the magnetron sputtering chamber; the chamber was evacuated to a pressure of less than 1×10 -3 After 1.0 Pa, high-purity argon gas is introduced, and the argon gas flow rate is adjusted to make the cavity pressure reach 2.0 Pa. The bias voltage is adjusted to -700 V, and the surface of the substrate is bias cleaned to remove impurities on the surface of the substrate;
[0027] (2) High-purity nitrogen was introduced, and the flow ratio of argon and nitrogen was controlled to be 10:1; the chamber pressure was adjusted to 1.1 Pa, the bias voltage was adjusted to -50 V, and the TiN transition layer was deposited by magnetron sputtering Ti target: the average current of Ti target was 0.85 A, and the target voltage was 600 V; the duty cycle of self-excited non-zero oscillation high-power micro-pulse magnetron sputtering power supply was 10%, and the pulse length was 125 us; the deposition time was 20 min, and the deposition thickness of TiN transition layer was 160 nm;
[0028] (3) Turn off and stop the nitrogen flow; adjust the chamber pressure to 1.0~1.1Pa, adjust the bias voltage to -50V, and magnetron sputter 3D network interpenetrating MoS2 target to deposit 3D network interpenetrating MoS2 thin film: the average current of 3D network interpenetrating MoS2 thin target is 0.39A, and the target voltage is 650V; the self-excited non-zero oscillation high-power micro-pulse magnetron sputtering power supply has a duty cycle of 10% and a pulse length of 125us; the deposition time is 120min, and the deposition thickness of the 3D network interpenetrating MoS2 thin film is 2.2um.
[0029] Compared with the 3D network interpenetrating molybdenum disulfide film prepared by medium frequency magnetron sputtering, the hardness of the 3D network interpenetrating molybdenum disulfide film prepared by vacuum self-excited non-zero position oscillation high-power micropulse magnetron sputtering in this embodiment is increased from 0.10 GPa to 3.55 GPa, and the elastic modulus is increased from 21.35 GPa to 62.65 GPa; the friction coefficient of the 3D network interpenetrating molybdenum disulfide film in a vacuum environment is 0.035, and the calculated wear rate is 8.61×10 -8 mm -3 / Nm; the friction coefficient in the atmospheric environment is 0.065, the friction life is not less than 100,000 cycles, and the calculated wear rate is 6.05×10 -7 mm -3 / Nm; the friction life measured in a vacuum environment is greater than 900,000 cycles, and the friction life measured in an atmospheric environment is greater than 100,000 cycles.
[0030] Example 2
[0031] (1) The substrate was ultrasonically cleaned with acetone and alcohol for 20-30 min to remove surface impurities and organic matter, then dried with nitrogen and placed on the sample holder of the magnetron sputtering chamber; the chamber was evacuated to a pressure of less than 1×10 -3 After 1.0 Pa, high-purity argon gas is introduced, and the argon gas flow rate is adjusted to make the cavity pressure reach 2.0 Pa. The bias voltage is adjusted to -800 V, and the surface of the substrate is bias cleaned to remove impurities on the surface of the substrate;
[0032] (2) High-purity nitrogen was introduced, and the flow ratio of argon and nitrogen was controlled to be 10:1; the chamber pressure was adjusted to 1.1 Pa, the bias voltage was adjusted to -80 V, and the TiN transition layer was deposited by magnetron sputtering Ti target: the average current of Ti target was 0.85A, and the target voltage was 600V; the duty cycle of self-excited non-zero oscillation high-power micro-pulse magnetron sputtering power supply was 10%, and the pulse length was 125us; the deposition time was 20min, and the deposition thickness of TiN transition layer was 160nm;
[0033] (3) Turn off the nitrogen flow; adjust the chamber pressure to 1.0~1.1Pa, adjust the bias voltage to -80V, and deposit 3D network interpenetrating MoS2 film by magnetron sputtering: the average current of 3D network interpenetrating MoS2 target is 0.42A, and the target voltage is 650V; the duty cycle of self-excited non-zero oscillation high-power micro-pulse magnetron sputtering power supply is 10%, and the pulse length is 83us; the deposition time is 120min, and the deposition thickness of 3D network interpenetrating MoS2 film is 3.1nm.
[0034] Compared with the 3D network interpenetrating MoS2 film prepared by medium frequency magnetron sputtering, the hardness of the 3D network interpenetrating MoS2 film prepared by vacuum self-excited non-zero position oscillation high-power micro-pulse magnetron sputtering in this embodiment is increased from 0.10 GPa to 2.76 GPa, and the elastic modulus is increased from 21.35 GPa to 48.59 GPa; the friction coefficient of the 3D network interpenetrating MoS2 film in a vacuum environment is 0.045, and the calculated wear rate is 9.24×10 -8 mm -3 / Nm; the friction coefficient in the atmospheric environment is 0.075, the friction life is not less than 100,000 cycles, and the calculated wear rate is 7.37×10 -7 mm -3 / Nm; the friction life measured in a vacuum environment is greater than 900,000 cycles, and the friction life measured in an atmospheric environment is greater than 100,000 cycles.
Claims
1. A method for preparing a 3D network interpenetrating molybdenum disulfide film using a self-excited non-zero oscillation high-power pulse technology, comprising the following steps: (1) The substrate was ultrasonically cleaned with acetone and alcohol for 20-30 min to remove surface impurities and organic matter; then it was blown dry with nitrogen and placed on the sample holder of the magnetron sputtering chamber, and the chamber was evacuated to a pressure of less than 1×10 -3 Pa; then introduce high-purity argon gas, adjust the argon gas flow rate to make the chamber pressure reach 2.0~3.0Pa, adjust the bias voltage to -700~-800V, and perform bias cleaning on the surface of the substrate to remove impurities on the surface of the substrate; (2) High-purity nitrogen was introduced, and the flow ratio of argon and nitrogen was controlled to be 10:1; the chamber pressure was adjusted to 1.0~1.3Pa, the bias voltage was adjusted to -50~-100V, and the TiN transition layer was deposited by self-excited non-zero oscillation high-power micro-pulse magnetron sputtering Ti target: the duty cycle of the self-excited non-zero oscillation high-power micro-pulse magnetron sputtering power supply was 10%, the pulse length was 125μs, the deposition time was 20~25min, and the deposition thickness of the TiN transition layer was 150~200nm; (3) Stop nitrogen flow, adjust the chamber pressure to 1.0~1.3 Pa, adjust the bias voltage to -50~-80 V, and use self-excited non-zero oscillation high-power micro-pulse magnetron sputtering to deposit 3D network interpenetrating MoS2 thin film. The duty cycle of the self-excited non-zero oscillation high-power micro-pulse magnetron sputtering power supply is 10%, and the pulse length is 83~125 μs. The deposition time is 120 min, and the deposition thickness of the 3D network interpenetrating MoS2 thin film is 2.2~3.1 um.
2. The method for preparing 3D network interpenetrating molybdenum disulfide thin film by self-excited non-zero oscillation high power pulse technology as claimed in claim 1, characterized in that: In step (1), the substrate is a stainless steel sheet or a single crystal silicon sheet.
3. The method for preparing 3D network interpenetrating molybdenum disulfide thin film by self-excited non-zero position oscillation high power pulse technology as claimed in claim 1, characterized in that: In step (2), the average current of the Ti target is 0.85A and the target voltage is 600V.
4. The method for preparing 3D network interpenetrating molybdenum disulfide thin film by self-excited non-zero oscillation high power pulse technology as claimed in claim 1, characterized in that: In step (3), the average current of the molybdenum disulfide target is 0.39~0.42A, and the target voltage is 650V.