Preparation method and application of infrared stealth fabric

By coating the MXene material prepared by etching on the fabric surface, the problem of complex and high cost of preparation of existing infrared stealth materials is solved, and an efficient and low-cost infrared stealth fabric is achieved, with good stealth effect and flat surface.

CN115787283BActive Publication Date: 2024-11-12BEIJING INST OF CLOTHING TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111263452.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-09-10
Filing Date
2021-10-28
Publication Date
2024-11-12
Estimated Expiration
2041-10-28

AI Technical Summary

Technical Problem

The preparation process of existing infrared stealth flexible materials is cumbersome and has high cost. The coating material has poor bonding properties with the coated material, and the infrared emissivity is high, making it difficult to achieve a good stealth effect.

Method used

MXene material is used to coat the fabric surface, and MXene solution is prepared by etching and coated on the fabric, combined with water washing and drying treatment to achieve a tight interface bond without additives and reduce infrared emissivity.

Benefits of technology

The preparation of infrared stealth fabrics is achieved, with simple process and low cost, flat coating layer without falling off, high infrared reflectivity and low infrared emissivity, which significantly improves the stealth effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005043187590000131
    Figure GDA0005043187590000131
  • Figure HDA0003427276410000011
    Figure HDA0003427276410000011
  • Figure HDA0003427276410000012
    Figure HDA0003427276410000012
Patent Text Reader

Abstract

The present invention provides an infrared stealth fabric and a preparation method thereof, comprising the following steps: coating MXene obtained by etching on the surface of the fabric, and drying to obtain the infrared stealth fabric of the present invention. The preparation method of the present invention has the advantages of simple preparation process, low preparation cost, convenient operation, etc., and the MXene in the prepared infrared stealth fabric is tightly combined with the fabric surface, and the MXene hardly falls off after repeated folding for several times, and the surface of the stealth fabric is flat after coating without bulging, and it has a high infrared reflectivity in the infrared band, and is a typical low infrared emissivity fabric.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an infrared stealth material, and in particular to a preparation method and application of an infrared stealth fabric. Background Art

[0002] Stealth technology is a technology that controls the signal characteristics of weapons such as aircraft, tanks, and ships to make them difficult to be discovered, identified, tracked, and attacked. It is aimed at detection technology. It mainly includes visible light stealth, infrared stealth, radar stealth, laser stealth, and acoustic stealth. The technical approaches to achieve stealth mainly include appearance design, stealth materials, and plasma stealth technology, among which stealth materials are an important technology with a wide range of applications, especially visible light-infrared stealth materials, which are a hot spot in current stealth technology research.

[0003] Infrared stealth flexible materials refer to various infrared stealth materials developed with fabrics as the center, often based on high-performance fiber fabrics. Stealth materials can reduce the detection rate and improve their own survival rate, and are an important part of stealth technology. According to the spectrum, they can be divided into acoustic, radar, infrared, visible light, and laser stealth materials. According to the use of materials, they can be divided into stealth coating materials and stealth structural materials.

[0004] MXene is a class of two-dimensional inorganic compounds, which are composed of transition metal carbides, nitrides or carbonitrides with a thickness of several atomic layers. It is usually obtained by removing the intermediate phase of MAX phase ceramics. MAX phase refers to M n+1 AX n (n = 1, 2 or 3), where M refers to transition metal, A represents III or IV main group elements (mainly Al, Ga, In, Ti, Si, Ge, Sn, Pb), and X is carbon, nitrogen or carbon-nitrogen elements. Because n can be 1, 2, or 3, the corresponding structure is M2X, M3X2 or M4X3, and the two-dimensional sheets are 211 phase, 312 phase and 413 phase, corresponding to different sheet thicknesses. In nature, only MXenes with oxygen, hydrogen, oxygen and fluorine as ends exist. Pure MXene without end groups cannot exist. MXene has good hydrophilicity and dispersibility due to the various functional groups on its surface, and can stably fuse with a variety of organic solvents in aqueous solution. MXene materials also have a special two-dimensional layered structure and ultra-high conductivity (conductivity can reach 7.3×10 4 S / m), it can be widely used in the field of wave absorption. MXene absorbs electromagnetic waves mainly through dielectric loss.

[0005] In the prior art, there is little research on infrared stealth flexible materials. In the preparation of infrared stealth flexible materials, a variety of ligands and adhesives need to be added. The preparation process is cumbersome and the preparation cost is high. The bonding between the coating material and the coated material is poor, and the infrared emissivity is high. Summary of the invention

[0006] Based on the above technical background, the inventors have made determined efforts and found that: by coating MXene on the surface of the fabric, an infrared stealth fabric material can be obtained without adding other additives, and the obtained stealth fabric material has a good interface bonding effect between the fabric surface and MXene, and there is almost no MXene shedding after repeated folding several times, and the surface of the obtained stealth fabric is smooth without bulging. It has a high infrared reflectivity in the infrared band and is a typical low infrared emissivity fabric with good stealth effect. At the same time, the preparation process of the stealth fabric material is simple and easy to operate.

[0007] A first aspect of the present invention is to provide an infrared stealth fabric, which is prepared by coating MXene on the surface of the fabric, and the MXene is prepared by etching MAX.

[0008] The second aspect of the present invention is to provide a method for preparing the infrared stealth fabric according to the first aspect of the present invention, the preparation method comprising the following steps:

[0009] Step 1, preparing MXene;

[0010] Step 2, coating the MXene prepared in step 1 on the surface of the fabric;

[0011] Step 3: preparing the infrared stealth fabric through post-processing.

[0012] The preparation method of the infrared stealth fabric provided by the present invention and the stealth fabric prepared thereby have the following advantages:

[0013] (1) The infrared stealth fabric of the present invention has a simple preparation process, low preparation cost and convenient operation;

[0014] (2) The infrared stealth fabric coating layer of the present invention is tightly bonded to the fabric and almost never falls off;

[0015] (3) After being coated with MXene, the infrared stealth fabric of the present invention has a smooth surface without bulging, and the coating thickness is extremely thin;

[0016] (4) The infrared stealth fabric of the present invention has a high infrared reflectivity in the infrared band and is a typical low infrared emissivity fabric. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1-a The surface morphology of the uncoated cotton cloth of Example 3 of the present invention is shown;

[0018] Figure 1-b The surface morphology of the cotton cloth after coating with MXene in Example 3 of the present invention is shown;

[0019] Figure 1-c The surface morphology of the cotton cloth coated with MXene and dried in Example 3 of the present invention is shown;

[0020] Figure 2 The infrared emissivity curves of the cotton cloth coated with MXene obtained in Examples 3 to 8 of the present invention are shown;

[0021] Figure 3 The XRD pattern of the product obtained in Example 1 of the present invention is shown. DETAILED DESCRIPTION

[0022] The present invention will be described in detail below, and the characteristics and advantages of the present invention will become clearer and more distinct with the description.

[0023] A first aspect of the present invention is to provide an infrared stealth fabric, which is prepared by coating MXene on the surface of the fabric, and the MXene is prepared by etching MAX.

[0024] In the present invention, the fabric is selected from cotton fabric, rayon fabric, polyester fabric, acrylic fabric or spandex fabric; preferably, the fabric is selected from cotton fabric, rayon fabric or acrylic fabric; more preferably, the fabric is cotton fabric.

[0025] In a preferred embodiment of the present invention, the fabric is a pre-treated fabric. It is found through experiments that after the pre-treated fabric is coated with MXene, its infrared reflectivity in the infrared band is greatly reduced, indicating that the stealth fabric made of the pre-treated fabric has a better stealth effect. The pre-treatment includes washing and drying.

[0026] The MXene is prepared by etching MAX, and the MAX phase is a new type of machinable ceramic material that has attracted much attention (for details on the preparation, structure and properties of the MAX phase, see (Zheng Yali, Zhou Yanchun, Feng Zhihai, Preparation, Structure, Properties and Development Trends of MAX Phase Ceramics, Aerospace Materials Technology, 2013, Issue 6, Pages 1-23)).

[0027] The MXene of the present invention is selected from one or more of Ti4N3, Ti3C2, Zr3C2, Ti2C, V4C3, Cr2C and W2C; preferably, the MXene is selected from one or more of Ti4N3, Ti3C2, Ti2C and W2C; more preferably, the MXene is selected from one or more of Ti3C2 and Ti2C.

[0028] The etchant is selected from one of HF, NH4HF2, LiF+HCl and NaOH, preferably selected from one of LiF+HCl and NaOH, more preferably LiF+HCl. LiF+HCl is a mixture of LiF and HCl.

[0029] The experiment found that after MXene was made into a solution and then coated on the surface of the fabric, a strong bonding force could be formed between the fabric and MXene, that is, the infrared stealth fabric described in the present invention does not need to add other adhesives or other additives, and MXene can be firmly adhered to the fabric surface. Especially when cotton fabric is used as the fabric and one or two of Ti3C2 and Ti2C are used as MXene, the bonding force between the cotton fabric and the coating is better. The obtained fabric was folded repeatedly several times, and the coating hardly fell off.

[0030] The coating layer of the present invention is composed of MXene, and the thickness of the coating layer is 10um to 200um, preferably 20um to 150um, and more preferably 60 to 140um. It can be seen that the thickness of the coating layer of the stealth material prepared by the present invention is extremely thin.

[0031] The coating amount of MXene in the present invention is 0.1 to 10 g / m 2 Preferably, the coating amount of MXene is 0.5 to 9 g / m 2 More preferably, the coating amount of MXene is 1 to 8 g / m 2 The coating amount of MXene in the present invention refers to the coating mass of MXene per unit area of ​​the fabric surface.

[0032] The number of layers of MXene is 1 to 20, preferably, the number of layers of MXene is 1 to 10, and more preferably, the number of layers of MXene is 1 to 5. MXene is a two-dimensional layered structure, and the number of layers of MXene refers to the number of layers of its layered structure.

[0033] The infrared stealth fabric of the present invention has a smooth surface after being coated with MXene, without bulging. It can be deduced from Kirchhoff's law that to prepare a material with low infrared emissivity, the material must have a higher reflectivity in the infrared band. MXene has metal-like properties, high surface carrier density, and high reflectivity. The reflectivity is also related to the surface condition of the material. The smoother the surface, the greater the reflectivity, and thus has a lower infrared emissivity. Therefore, in the present invention, using MXene as a coating layer and the smooth surface of the fabric after coating are both conducive to reducing the reflectivity in the infrared band.

[0034] The infrared emissivity of the infrared stealth fabric is 0.1-0.5 at 3-5 μm, and the infrared emissivity at 8-14 μm is 0.1-0.5.

[0035] The infrared stealth fabric of the present invention is prepared by a method comprising the following steps:

[0036] Step 1, preparing MXene;

[0037] Step 2, coating the MXene prepared in step 1 on the surface of the fabric;

[0038] Step 3: preparing the infrared stealth fabric through post-processing.

[0039] In step 2, the MXene is made into a solution and then coated on the surface of the fabric. The concentration of the MXene solution is 5 to 8 mg / mL, preferably 5.5 to 7.5 mg / mL, and more preferably 5.9 to 7.2 mg / mL.

[0040] The second aspect of the present invention is to provide a method for preparing the infrared stealth fabric according to the first aspect of the present invention, the preparation method comprising the following steps:

[0041] Step 1, preparing MXene;

[0042] Step 2, coating the MXene prepared in step 1 on the surface of the fabric;

[0043] Step 3: preparing the infrared stealth fabric through post-processing.

[0044] This step is described and illustrated in detail below.

[0045] Step 1: Prepare MXene.

[0046] The MXene is prepared by etching MAX with an etchant. The MXene of the present invention is selected from one or more of Ti4N3, Ti3C2, Zr3C2, Ti2C, V4C3, Cr2C and W2C; preferably, the MXene is selected from one or more of Ti4N3, Ti3C2, Ti2C and W2C; more preferably, the MXene is selected from one or more of Ti3C2 and Ti2C.

[0047] The etchant is selected from one of HF, NH4HF2, LiF+HCl and NaOH. HF is highly dangerous and difficult to store, while NH4HF2 is highly toxic and easily decomposes into toxic fluoride, nitrogen oxide and ammonia gas in hot water, which is extremely harsh on experimental synthesis conditions. In the present invention, the etchant is preferably selected from one of LiF+HCl and NaOH, more preferably LiF+HCl. Using a mixture of LiF and HCl as an etchant has the advantages of mild synthesis process and little environmental pollution.

[0048] First, LiF and HCl are placed in a reactor, and then the MAX phase is slowly added into the reactor. The amount of hydrochloric acid used is not limited as long as it can completely dissolve LiF.

[0049] The mass ratio of MAX to LiF is 3: (3-10), preferably, the mass ratio of MAX to LiF is 3: (7-9), and more preferably, the mass ratio of MAX to LiF is 3: 8. It is found through experiments that when the mass ratio of MAX to LiF is 3: (5-10), the mixture of LiF and HCl has a better etching effect on MAX.

[0050] The etching reaction of the present invention is carried out by heating in an oil bath, and stirring is performed during the reaction, preferably magnetic stirring.

[0051] The etching reaction temperature is 30°C to 50°C, preferably 35°C to 45°C, and more preferably 40°C. The etching reaction time is 24 to 72 hours, preferably 45 to 50 hours, and more preferably 48 hours. The inventors have found that when the etching temperature is 30°C to 50°C and the etching time is 40 to 55 hours, the etching reaction can achieve good etching effects at a higher efficiency.

[0052] After etching is completed, the etching reaction system is taken out of the reactor and washed multiple times, preferably centrifugally. The purpose of centrifugation is to remove impurities in the reaction system. The number of centrifugation is preferably 2 to 5 times, more preferably 3 times. After centrifugation, multilayer MXene is obtained, and the obtained multilayer MXene aqueous solution is filled with inert gas and refrigerated for subsequent use.

[0053] In the present invention, the multilayer MXene has 10 to 30 layers, preferably 10 to 20 layers, and more preferably 10 to 15 layers.

[0054] Preferably, the multilayer MXene is subjected to ultrasonic exfoliation and then centrifugal washing, and the supernatant is taken to obtain the few-layer MXene. The few-layer MXene aqueous solution is filled with inert gas and refrigerated for subsequent use.

[0055] According to the present invention, the few-layer MXene is 1 to 10 layers, preferably 1 to 7 layers, and more preferably 1 to 5 layers.

[0056] Step 2: Coat the MXene prepared in step 1 on the surface of the fabric.

[0057] According to the present invention, the fabric is selected from cotton fabric (i.e. cotton cloth), rayon fabric, polyester fabric, acrylic fabric or spandex fabric; preferably, the fabric is selected from cotton fabric, rayon fabric or acrylic fabric; more preferably, the fabric is cotton fabric.

[0058] MXene is a material with good wave-absorbing properties. The inventors have found that by coating it on the surface of a fabric, a flexible fabric stealth material with good wave-absorbing properties can be obtained. In particular, when the coating material is Ti3C2 and the fabric is cotton fabric, no other additives need to be added. There is a good interface between the cotton fabric and Ti3C2, and the coating has almost no shedding after repeated folding.

[0059] According to a preferred embodiment of the present invention, the fabric is pre-treated before coating, and more preferably, the pre-treatment includes washing and drying. It is found through experiments that after the fabric is pre-treated, the infrared emissivity of the infrared stealth fabric is lower and the infrared stealth effect is better.

[0060] There are hydrogen bonds on both the fabric surface and the MXene surface, especially on the cotton fabric surface. After MXene is coated on the cotton fabric surface, the MXene and the cotton fabric are bonded through hydrogen bonds and electrostatic interactions, making the MXene and the cotton fabric well bonded.

[0061] The MXene is made into a solution and then coated on the surface of the fabric. The solvent is preferably selected from one of water, ethanol, methanol and acetone, more preferably water.

[0062] The concentration of the MXene solution is 5 to 8 mg / mL, preferably 5.5 to 7.5 mg / mL, and more preferably 5.9 to 7.2 mg / mL. The experiment found that the concentration of the MXene solution affects the infrared reflectivity of the obtained stealth fabric. The lower the concentration of the MXene solution, the more evenly it is coated on the surface of the fabric, the smoother the surface of the obtained stealth fabric, and the lower its infrared emissivity. When the concentration of the MXene solution is 5 to 8 mg / mL, the MXene is more evenly coated on the surface of the fabric, the better the interface bonding between the obtained stealth fabric MXene and the fabric surface, and the less likely the MXene will fall off the fabric surface.

[0063] The coating amount of MXene in the present invention is 0.1 to 10 g / m 2 Preferably, the coating amount of MXene is 0.5 to 9 g / m 2 More preferably, the coating amount of MXene is 1 to 8 g / m 2 The coating amount of MXene in the present invention refers to the coating mass of MXene per unit area of ​​the fabric surface.

[0064] The experiment found that the coating amount of MXene will affect the infrared reflectivity of infrared stealth fabrics. As the coating amount of MXene increases, the infrared reflectivity of infrared stealth fabrics gradually decreases, and the stealth effect becomes better and better. When the coating amount of MXene is 0.1-10g / m 2The infrared reflectivity of the obtained stealth fabric is relatively low, especially when the coating amount of MXene is 1-8 g / m 2 When , the infrared reflectivity of the infrared stealth fabric is the lowest and the stealth effect is the best.

[0065] The number of MXene layers is 1 to 20 layers, preferably, the number of MXene layers is 1 to 10 layers, and more preferably, the number of MXene layers is 1 to 5 layers. The inventors found that the number of MXene layers coated on the surface of the fabric will also affect the stealth effect of the obtained stealth fabric. The fewer the number of MXene layers, the lower the infrared reflectivity of the stealth fabric, and the better the stealth effect. When the number of MXene layers is 1 to 5 layers, the infrared reflectivity of the obtained stealth fabric has a lower infrared reflectivity in the 3 to 5 μm and 8 to 14 μm infrared bands, and the stealth effect is good.

[0066] Step 3: preparing the infrared stealth fabric through post-processing.

[0067] The post-treatment of the present invention includes drying, preferably drying in a vacuum oven. Vacuum drying can make the coating coated on the fabric surface more firmly bonded to the fabric surface. This is mainly because drying is carried out under a vacuum state, avoiding the generation of residual bubbles between the coating and the fabric surface, so that the coating is more firmly attached to the fabric surface.

[0068] The coating layer of the infrared stealth fabric prepared by the present invention is composed of MXene, and the thickness of the coating layer is 10um to 200um, preferably 20um to 150um, and more preferably 60 to 140um. It can be seen that the thickness of the coating layer of the stealth material prepared by the present invention is extremely thin.

[0069] The infrared stealth fabric prepared by the invention has an infrared emissivity of 0.1 to 0.5 at 3 to 5 μm and an infrared emissivity of 0.1 to 0.5 at 8 to 14 μm.

[0070] The beneficial effects of the present invention are:

[0071] (1) The preparation method of the infrared stealth fabric of the present invention avoids the addition of other additives during the preparation process, making the preparation method simple and low in cost;

[0072] (2) The preparation method of the infrared stealth fabric of the present invention has low requirements on preparation equipment and high feasibility of industrial scale-up;

[0073] (3) After the infrared stealth fabric of the present invention is coated with MXene, the surface is smooth without bulging, and there is a good interface bonding effect between MXene and the fabric surface. The fabric exhibits excellent flexibility and mechanical properties, and the coating hardly falls off after repeated folding.

[0074] (4) The infrared stealth fabric described in the present invention has a low infrared emissivity in the infrared bands of 3-5 μm and 8-14 μm, and the infrared emissivity decreases with the increase of the coating dosage. Its emissivity in the infrared bands of 3-5 μm and 8-14 μm is 0.1-0.5.

[0075] Example

[0076] The present invention is further described below by means of specific examples. These embodiments are only intended to illustrate the present invention but are not intended to limit the scope of the present invention.

[0077] Example 1 Preparation of multilayer MXene (multilayer may be referred to as m-MXene)

[0078] Put 4g LiF and 50mL concentrated hydrochloric acid into the reactor, slowly add 1.5g Ti3AlC2, put the reactor into a 40℃ oil bath, and react for 48h under magnetic stirring. Take out the sample, centrifuge and wash it 3 times with deionized water to remove impurities, and obtain multilayer Ti3C2. Fill the multilayer Ti3C2 aqueous solution with inert gas and refrigerate it for use.

[0079] Example 2 Preparation of few-layer MXene (few-layer can be called d-MXene)

[0080] The preparation process of Example 1 was repeated, except that after obtaining the multi-layer Ti3C2, ultrasonic peeling was performed, and the supernatant was centrifuged again to obtain the few-layer Ti3C2. The few-layer Ti3C2 aqueous solution was filled with inert gas and refrigerated for use.

[0081] Example 3

[0082] Take 8×8cm cotton cloth and stick it on the metal plate. The surface is flat and free of debris. Take 1mL of MXene with a concentration of 7.18mg / mL (solvent is deionized water) and evenly coat it with a few layers (1 to 5 layers) on the cotton cloth, and then dry it in a vacuum oven. The surface morphology of the cotton cloth before coating, after coating, and after coating and drying are as follows: Figure 1-a , Figure 1-b and Figure 1-c As shown by Figure 1-a , Figure 1-b and Figure 1-c It can be seen that the surface of the cotton cloth before coating, after coating and after drying is flat, the coating is uniform and there is no bulging. The coating layer thickness is 20 μm.

[0083] Example 4

[0084] The preparation process of Example 3 was repeated, except that 3 mL of MXene with a concentration of 7.18 mg / mL and a few layers (1 to 5 layers) were uniformly coated on the cotton cloth. The coating layer thickness was 60 μm.

[0085] Example 5

[0086] The preparation process of Example 3 was repeated, except that 5 mL of MXene with a concentration of 7.18 mg / mL and a few layers (1 to 5 layers) were uniformly coated on the cotton cloth. The coating layer thickness was 100 μm.

[0087] Example 6

[0088] The preparation process of Example 3 was repeated, except that 7 mL of MXene with a concentration of 7.18 mg / mL and a few layers (1 to 5 layers) were uniformly coated on the cotton cloth. The coating layer thickness was 140 μm.

[0089] Example 7

[0090] The preparation process of Example 3 was repeated, except that 7 mL of MXene with a concentration of 7.18 mg / mL and multiple layers (10 layers) were uniformly coated on cotton cloth. The coating layer thickness was 140 μm.

[0091] Example 8

[0092] The preparation process of Example 4 was repeated, except that 8×8 cm of washed cotton cloth was air-dried and then adhered to the metal plate before coating. The coating layer thickness was 60 μm.

[0093] Example 9

[0094] Take 6mL of 7.18mg / mL MXene with few layers (1 to 5 layers) and add 1.2mL of deionized water to dilute it. Take 8×8cm cotton cloth that has been washed and dried and stick it on the metal plate. The surface is flat and free of debris. Take the above 1.2mL of diluted few layers of MXene and evenly coat it on the cotton cloth, and then dry it in a vacuum oven. The coating thickness is 20μm.

[0095] Example 10

[0096] The preparation process of Example 9 was repeated, except that 2.4 mL of diluted few layers (1 to 5 layers) of MXene were uniformly coated on the washed cotton cloth. The coating layer thickness was 40 μm.

[0097] Embodiment 11

[0098] The preparation process of Example 9 was repeated, except that 3.6 mL of diluted few layers (1 to 5 layers) of MXene were uniformly coated on the washed cotton cloth. The coating layer thickness was 80 μm.

[0099] Comparative Example

[0100] Comparative Example 1

[0101] The preparation process of Example 3 was repeated, except that the coating material was 3.6 mL of a mixture of aluminum powder and ethanol at a concentration of 5.98 mg / mL, and the coating layer thickness was 80 μm.

[0102] Experimental example

[0103] Experimental Example 1 Infrared thermal emissivity test

[0104] The infrared thermal emissivity test of the above-mentioned embodiments 3 to 11 and comparative example 1 was carried out using an infrared detector. The infrared thermal emissivity test of the cotton cloth coated in the above-mentioned embodiments 3 to 11 and comparative example 1 was carried out using the infrared emission bands of 3 to 5 μm and 8 to 14 μm. In the infrared detection band, the infrared detector mainly detects the infrared radiation intensity of the target. The greater the infrared radiation intensity, the easier it is to be detected, and the greater the probability of the target being discovered. The test results are shown in Tables 1 and Figure 2 As shown:

[0105] Table 1 Infrared emissivity test results

[0106]

[0107] pass Figure 2 It can be seen that with the increase in the amount of MXene used, the infrared emissivity tends to decrease. The infrared emissivity of cotton cloth coated with 7mL multi-layer MXene is higher than that of cotton cloth coated with 7mL few-layer MXene, indicating that the stealth effect of the stealth fabric prepared after coating with few layers of MXene is better. It can also be seen that the infrared emissivity of the washed cotton cloth after coating is lower than that of the unwashed cotton cloth, indicating that the stealth effect of the stealth fabric made of pre-treated cotton cloth is better.

[0108] It can be seen from Table 1 that the emissivity of the cotton cloth coated with aluminum powder in the 3-5 μm infrared band is 0.297, and the infrared emissivity in the 8-14 μm band is 0.373. Its infrared emissivity is basically higher than that of the cotton cloth coated with MXene, indicating that the stealth effect of the stealth fabric obtained after coating with MXene is better than that of the stealth fabric obtained after coating with aluminum powder, and the coating layer of aluminum powder is thicker.

[0109] It can be seen from Table 1 above that with the increase of the MXene coating amount, the infrared emissivity becomes lower and lower. The infrared emissivities of the coated cotton cloth prepared in Example 9 are 0.223 and 0.220, respectively, which are better than the stealth fabric made of traditional coating materials. In addition, the coating thickness of the present application is extremely thin. When 3.6 mL of MXene is coated in Example 11 of the present application, the emissivity in the 3-5 μm infrared band is only 0.142, and the infrared emissivity in the 8-14 μm band is 0.172, indicating that the stealth material prepared by the present invention is a typical low infrared emissivity fabric.

[0110] Experimental Example 2 XRD test

[0111] XRD performance test was performed on Ti3AlC2 and the prepared Ti3C2 in Example 1. The test results are as follows: Figure 3 shown.

[0112] Depend on Figure 3 It can be seen that compared with the Ti3AlC2 spectrum, the characteristic absorption peak of Al in Ti3C2 disappears. At the same time, it can be seen that the (002) peak in the Ti3C2 spectrum shifts to a small angle, indicating that the etching is successful.

[0113] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing infrared stealth fabric, It is characterized in that The infrared stealth fabric is made by coating MXene on the fabric surface, and the MXene is made by etching MAX; MXene is selected from Ti 4 N 3 、Ti 3 C 2 、Ti 2 C and W 2 One or more of C; The fabric is selected from cotton fabric, rayon fabric or acrylic fabric; The coating amount of MXene on the fabric surface is 0.1-10 g / m 2 ; The number of MXene layers ranges from 1 to 20; The preparation method comprises the following steps: Step 1, preparing MXene; Step 2, coating the MXene prepared in step 1 on the surface of the fabric; Step 3, after post-processing, an infrared stealth fabric is obtained, wherein the infrared emissivity of the infrared stealth fabric is 0.1 to 0.5 at 3 to 5 μm, and the infrared emissivity of the infrared stealth fabric is 0.1 to 0.5 at 8 to 14 μm; In step 1, The MXene is prepared by etching MAX with an etchant, wherein the etchant is LiF+HCl; The mass ratio of MAX to LiF is 3:(3-10); The etching temperature is 30°C to 50°C; The etching is carried out under magnetic stirring, and the stirring time is 24 to 72 hours; After etching, washing is performed to obtain a multi-layer MXene, the number of which is 10 to 30 layers; the obtained multi-layer MXene is subjected to ultrasonic exfoliation and then washed to obtain a few-layer MXene, the number of which is 1 to 10 layers; In step 2, The MXene is made into a solution and then coated on the surface of the fabric; The concentration of the MXene solution is 5.5-7.5 mg / mL.

2. The preparation method according to claim 1, It is characterized in that In step 2, the fabric is pre-treated before coating.

3. The preparation method according to claim 2, It is characterized in that In step 2, the pretreatment includes washing and drying.