Carbon fiber precursor oil and preparation method thereof
By modifying the combination of silicone and other surfactants, carbon fiber raw silk oil agent is prepared, which solves the problem of high fiber breakage and disconnection number of fibers during pre-oxidation, improves fiber density and strand strength, and improves fiber Adhesion and thermal stability.
Patent Information
- Application Number
- CN202211445122.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-18
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-11-18
AI Technical Summary
The existing carbon fiber raw silk oil agents cause fiber disconnection, high number of yarn and yarn and low density during the pre-oxidation process, and the water dispersion of dimethylsiloxane is poor, which affects the adhesion of polyacrylonitrile fibers.
Using modified silicone, fatty alcohol polyoxyethylene ether, non-ionic antistatic agent, fatty acid polyoxyethylene ester and antioxidant, carbon fiber raw silk oil agent is prepared through mechanical emulsification to control the structure and ammonia of the modified silicone The value of the content is to form a stable aqueous emulsion, which enhances the adhesion and dispersion of the fibers.
Effectively reduce the number of broken wires and unblocked wires of pre-oxidized fibers, improve fiber density, improve fiber smoothness and thermal stability, and enhance the bundled wire strength and line density of carbon fibers.
Smart Images

Figure CN115787305B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a carbon fiber precursor oil agent and a preparation method thereof. Background Art
[0002] Carbon fiber has excellent properties such as high strength, low density, anti-friction, high temperature resistance, corrosion resistance, electrical conductivity, and thermal conductivity. Therefore, it is often used as a reinforcing material and compounded with resins, metals, ceramics, etc. to manufacture advanced composite materials, which can be widely used in military fields such as aerospace and civil fields such as construction and automobiles. Carbon fiber can be made from polyacrylonitrile fiber, asphalt fiber, viscose fiber or phenolic fiber by carbonization. At present, most of the carbon fiber preparation methods adopt the following process: heating the raw silk in the presence of oxygen at 200-400℃ to convert it into refractory fiber, and then carbonizing and graphitizing it in an inert atmosphere above 1000℃ to obtain carbon fiber with excellent mechanical properties.
[0003] During the pre-oxidation stage, the structure of the carbon fiber precursor undergoes the evolution process of the tow structure-semi-molten stacking structure-lamellar divergence structure. In the early stage of pre-oxidation, the latter section and the middle section of pre-oxidation present a semi-molten stacking structure, which is a sensitive area for defect formation. Large structural defects such as hollow and parallel wire phenomena appear in the early and middle stages of the precursor pre-oxidation process. The obtained carbon fiber has more double-bundle adhesion structures, more macroporous structural defects inside the carbon fiber, and some hollow structures appear, with coarse and sparse lamellar textures. The pre-oxidized silk has a more obvious "skin-core" structure, with a dense silk surface and a loose core, and large voids appear. This defect will be brought into the carbon fiber, causing its performance to deteriorate. It is generally believed that the use of oils to protect the precursor fiber bundles can effectively reduce surface defects and the generation of hair.
[0004] Carbon fiber oil is an important auxiliary agent in the production process of carbon fiber. It provides effective protection and lubrication for carbon fiber during spinning, pre-oxidation and low-temperature carbonization. Therefore, high-quality oil is a necessary condition for high-quality carbon fiber. Its performance is mainly affected by the silicone oil used. At present, the silicone oil used in oil in China is dimethylsiloxane, but its characteristic is that it is insoluble in water. Even if an emulsifier is used and mechanical emulsification method is adopted, it is difficult to make a very stable water emulsion.
[0005] In order to improve the dispersibility of dimethylsiloxane in water and its adhesion to polyacrylonitrile fibers, dimethylsiloxane needs to be modified. Currently, modified silicone oils include amino-modified silicone oils, epoxy-modified silicone oils, polyether-modified silicone oils, etc. Among them, amino-modified silicone oils are widely welcomed due to their good hydrophilicity, emulsification and film-forming properties, but their adhesion to polyacrylonitrile fibers is poor, resulting in low oiling rate and poor uniformity of the oil agent, and the pre-oxidized fibers are prone to broken and woolen yarns, and the number of parallel yarns is high and the density is low. Summary of the invention
[0006] Purpose of the invention: In view of the defects of the prior art, the purpose of the present invention is to provide a carbon fiber raw fiber oil agent and a preparation method thereof, which can reduce pre-oxidized fiber breakage and yarn breakage, reduce the number of pre-oxidized fiber strands and increase fiber density through uniform oiling.
[0007] Technical solution:
[0008] A carbon fiber precursor oil agent, comprising modified siloxane, fatty alcohol polyoxyethylene ether, nonionic antistatic agent, fatty acid polyoxyethylene ester, antioxidant and deionized water;
[0009] The modified siloxane is a compound of formula I:
[0010]
[0011] Wherein m=5-10, n=50-60.
[0012] The raw silk oil can reduce friction, lower the dynamic friction between fiber and metal, and adjust the dynamic and static friction coefficients between fibers, that is, it handles the relationship between smoothness, fiber separation and bundling well; it has good adsorption and can be evenly distributed on the fiber surface; it has good thermal stability and has no effect on the fiber color; the raw silk is fully pre-oxidized, and the strength of the fiber bundle after carbonization is high.
[0013] During the carbonization process, the precursor silk has numerous holes and cracks of varying sizes due to the uneven structure caused by the mutual diffusion of solvent and precipitant. The precursor silk oil provided by the present invention solves the problem of inconsistent internal and external structures of the precursor silk, and effectively eliminates the "skin-core" structure of the oiled precursor silk after pre-oxidation; by coating the organic polymer, a uniform protective film can be formed on the surface of the precursor silk, effectively solving the problem of uneven antistatic properties of the precursor silk.
[0014] Furthermore, based on the total mass being 100%, the mass percentage of each component is:
[0015]
[0016] The balance was deionized water.
[0017] Furthermore, the preparation method of the modified siloxane is: under nitrogen protection, cyclosiloxane, aminosilane, catalyst and end-capping agent are mixed, gradually heated to 150-160°C, reacted for 20-24 hours, heated to 180-185°C, reacted for 3-5 minutes, then cooled and filtered to obtain the modified siloxane.
[0018] The modified siloxane obtained by controlling the reaction conditions has strong compatibility with water and can be used to obtain a stable aqueous emulsion through mechanical emulsification; it contains a high ammonia value and still has a large number of grafting sites in the structure, which can be further grafted and modified.
[0019] The modified siloxane has a viscosity of 5000-7000 mPa·S and an ammonia value of 0.5-0.6 meq / g.
[0020] In the method, the structure and amine value of the prepared modified siloxane are controlled by adding a catalyst and a capping agent and controlling the reaction temperature and time.
[0021] Furthermore, the cyclosiloxane is selected from one of hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane or dodecamethylcyclohexasiloxane; and the aminosilane is N-aminoethyl-3-aminopropylmethyldimethoxysilane.
[0022] Furthermore, the catalyst is selected from one of sodium hydroxide, potassium hydroxide, sodium methoxide, tetramethylammonium hydroxide or tetramethylguanidine; and the capping agent is hexamethyldisiloxane.
[0023] Furthermore, the mass ratio of the cyclosiloxane, aminosilane and end-capping agent is (25-35):(1-5):(0.5-1).
[0024] The structure and the amino value of the prepared modified siloxane are controlled by controlling the mass ratio of the cyclosiloxane and the aminosilane to the end-capping agent.
[0025] The method for preparing a carbon fiber precursor oil comprises the following steps:
[0026] (1) Adding fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester, nonionic antistatic agent and antioxidant into a stirred tank, stirring at 50-55° C. for 1-2 hours, and preparing a uniform composite emulsion for use;
[0027] (2) slowly adding the modified siloxane into a high shear emulsifier, starting stirring, slowly adding the pre-prepared composite emulsifier into the emulsifier, adjusting the temperature at 40-50° C., and after all the composite emulsifiers are added, adding deionized water dropwise thereto, adjusting the pH to 4.5-5.5, controlling the stirring speed to 2800-3200 r / min, stirring time to 100-140 minutes, stirring evenly, cooling to room temperature, and filtering to obtain a white emulsion, which is the carbon fiber precursor oil agent.
[0028] In the step (1), fatty alcohol polyoxyethylene ether and fatty acid polyoxyethylene ester are added, a part of which is used as an emulsifier and surfactant for the raw silk silicone oil, and a part of which undergoes an epoxycyclopropane addition reaction. In the step (2), the modified siloxane is further modified to link epoxy groups and carboxyl groups and graft hydrophilic polyether segments.
[0029] The raw silk oil prepared by the method has good washability and is easy to be washed off from the fiber; has good thermal stability and has no effect on the color of the fiber; has a neutral pH and is non-corrosive to equipment; is non-toxic, has no special smell, and has no irritation to the skin; is easy to prepare, convenient to use, safe and effective.
[0030] Furthermore, the general formula of the fatty alcohol polyoxyethylene ether in step (1) is RO(CH2CH2O)xH, wherein x=10-20, and R is a straight-chain or branched saturated alkane with 12-18 carbon atoms; the structural formula of the fatty acid polyoxyethylene ester is RCOO(EO)yH, wherein y=3-40, and R is a straight-chain or branched hydrocarbon with 4-20 carbon atoms.
[0031] Fatty acid polyoxyethylene ester is a nonionic surfactant with good surface activity such as emulsification, solubilization, wetting, dispersion, softness and antistatic, and is non-toxic and non-irritating. It is widely used in the industries of cosmetics, medicine, food, pesticides, papermaking, etc. It can be used as a thickener for shampoo and hair dye emulsion, a wetting agent for skin care cream, a solubilizing agent for essence and essential oil, a sunscreen and pearlescent agent for cosmetics, and can also be used as an emulsifier for pesticides, herbicides, and a softener in the papermaking industry. The present invention is compounded with fatty acid polyoxyethylene ester to be applied to raw silk oil.
[0032] A portion of fatty alcohol polyoxyethylene ether and fatty acid polyoxyethylene ester undergoes epoxy cyclopropane addition reaction to further modify the modified siloxane, linking epoxy groups, carboxyl groups and grafting hydrophilic polyether segments to make the modified silicone oil more water-soluble and dispersible, making the prepared raw silk oil more uniform and stable, and enhancing its adhesion ability to polyacrylonitrile fibers.
[0033] A part of fatty alcohol polyoxyethylene ether and fatty acid polyoxyethylene ester are compounded to obtain an emulsion that is uniform, stable and easy to store; it has a synergistic effect, so that the prepared raw silk oil has a good dispersion effect and stronger water solubility, and improves the oiling rate and uniformity of the raw silk oil.
[0034] Furthermore, in step (1), the nonionic antistatic agent is selected from one of glycerol stearate, fatty acid polyol ester or ethanolamide.
[0035] Adding the antistatic agent can enable the prepared raw silk oil to prevent static charges from accumulating on the fibers.
[0036] Furthermore, in step (1), the antioxidant is selected from one or a mixture of antioxidant 1076, antioxidant 1035 or phenolic antioxidant BHT.
[0037] Beneficial effects:
[0038] (1) In the method for preparing the carbon fiber precursor oil provided by the present invention, the structure and amine value of the modified siloxane obtained by the reaction are controlled by controlling the reaction conditions of the modified siloxane and the mass ratio of the raw materials and the end-capping agent.
[0039] (2) The modified siloxane used in the preparation method of the carbon fiber precursor oil provided by the present invention has strong compatibility with water and can be used to prepare a stable aqueous emulsion through mechanical emulsification; it contains a high ammonia value and still has a large number of grafting sites in the structure, which can be further grafted and modified.
[0040] (3) In the preparation method of the carbon fiber precursor oil provided by the present invention, fatty alcohol polyoxyethylene ether and fatty acid polyoxyethylene ester are used, wherein a part of the fatty alcohol polyoxyethylene ether and fatty acid polyoxyethylene ester are subjected to an epoxycyclopropane addition reaction to further modify the modified silicone, linking epoxy groups, carboxyl groups and grafting hydrophilic polyether segments to make the modified silicone oil have stronger water solubility and dispersibility, making the prepared precursor oil more uniform and stable, and enhancing its adhesion to polyacrylonitrile fiber; a part of the fatty alcohol polyoxyethylene ether and fatty acid polyoxyethylene ester are compounded to obtain an emulsion that is uniform, stable and easy to store; there is a synergistic effect, so that the prepared precursor oil has good dispersion effect and stronger water solubility, which can effectively enhance the oiling rate and uniformity of the precursor oil.
[0041] (4) The carbon fiber precursor oil provided by the present invention can reduce the breakage and wool of pre-oxidized fibers by evenly applying the oil, and can also reduce the number of pre-oxidized fibers and increase the fiber density.
[0042] (5) The raw silk oil provided by the present invention promotes the compactness of the fiber, enhances the linear density of the fiber, improves the heat release performance of the fiber, reduces the starting temperature of the exothermic reaction of the raw silk during the carbonization process, improves the concentrated release of reaction heat, reduces the reaction heat, increases the tensile strength of the carbon fiber, and reduces the broken wire rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 is the infrared spectrum of modified siloxane-1.
[0044] Figure 2 This is the drying infrared spectrum of modified siloxane-1.
[0045] Figure 3 This is the mass spectrometry of modified siloxane-1.
[0046] Figure 4 This is the thermal decomposition mass spectrum of modified siloxane-1. DETAILED DESCRIPTION
[0047] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0048] L656 is a non-reactive amino-modified polydimethylsiloxane with a high ammonia value purchased from Guangzhou Lai Ke Bao New Material Technology Co., Ltd.; L653 is a non-reactive amino-modified polydimethylsiloxane with a low ammonia value purchased from Guangzhou Lai Ke Bao New Material Technology Co., Ltd.; and Japanese Takemoto Oil Agent J-OA was purchased from Jilin Chemical Fiber Group Co., Ltd. The remaining reagents and equipment are conventional reagents and equipment in this technical field.
[0049] Preparation of modified siloxane-1
[0050] By weight, 35 parts of hexamethylcyclotrisiloxane, 1 part of N-aminoethyl-3-aminopropylmethyldimethoxysilane, 0.5 parts of 1 mol / L sodium hydroxide methanol solution and 0.5 parts of hexamethyldisiloxane were mixed under nitrogen protection, gradually heated to 160° C., reacted for 24 hours, then heated to 185° C., reacted for 5 minutes, then cooled and filtered to obtain the modified siloxane-1. The modified siloxane-1 has an amine value of 0.57 meq / g, a viscosity of 6237 mPa·s, and an HLB value of 13.
[0051] Preparation of modified siloxane-2
[0052] The preparation method is basically the same as that of modified siloxane-1, except that the components are changed to 25 parts of decamethylcyclopentasiloxane, 3 parts of N-aminoethyl-3-aminopropylmethyldimethoxysilane, 0.5 parts of tetramethylguanidine and 1 part of hexamethyldisiloxane. The modified siloxane-1 has an amine value of 0.52 meq / g, a viscosity of 5769 mPa·s and an HLB value of 13.
[0053] Preparation of modified siloxane-3
[0054] The preparation method is basically the same as that of modified siloxane-1, except that the components are changed to 30 parts of octamethylcyclotetrasiloxane, 5 parts of N-aminoethyl-3-aminopropylmethyldimethoxysilane, 0.5 parts of 1 mol / L potassium hydroxide methanol solution and 1 part of hexamethyldisiloxane. The modified siloxane-1 has an amine value of 0.54 meq / g, a viscosity of 6032 mPa·s and an HLB value of 13.
[0055] Example 1
[0056] Prepare the raw silk oil according to the following steps:
[0057] (1) Adding fatty alcohol polyoxyethylene ether AEO-9, fatty acid polyoxyethylene ester OEO-115, glycerol stearate and antioxidant 1076 into a stirred tank, stirring at 55° C. for 2 hours, and preparing a uniform composite emulsion for use;
[0058] (2) slowly adding the modified siloxane-1 into a high shear emulsifier, starting stirring, slowly adding the pre-prepared composite emulsifier into the emulsifier, adjusting the temperature at 50°C, and after all the composite emulsifiers have been added, adding an appropriate amount of deionized water, controlling the stirring speed to 3200 r / min, the stirring time to 140 minutes, adjusting the pH value to 5, stirring evenly, cooling to room temperature, filtering and packaging, and obtaining a white emulsion, which is the carbon fiber precursor oil agent.
[0059] Wherein, taking the total mass as 100%, the mass percentage of each component is:
[0060]
[0061] The balance was deionized water.
[0062] Example 2
[0063] The same as Example 1, except that the components and mass percentages are changed to:
[0064]
[0065]
[0066] The balance was deionized water.
[0067] Example 3
[0068] The same as Example 1, except that the components and mass percentages are changed to:
[0069]
[0070] The balance was deionized water.
[0071] Example 4
[0072] The same as Example 1, except that the mass percentage of each component is changed to:
[0073]
[0074] The balance was deionized water.
[0075] Example 5
[0076] The same as Example 1, except that the mass percentage of each component is changed to:
[0077]
[0078] The balance was deionized water.
[0079] Example 6
[0080] The same as Example 1, except that the mass percentage of each component is changed to:
[0081]
[0082] The balance was deionized water.
[0083] Comparative Example 1
[0084] The same as Example 1, except that the modified siloxane is changed to L656.
[0085] Comparative Example 2
[0086] The same as Example 1, except that the modified siloxane is changed to L653.
[0087] Comparative Example 3
[0088] The process is basically the same as Example 1, except that fatty acid polyoxyethylene ester OEO-115 is replaced by an equal amount of fatty alcohol polyoxyethylene ether AEO-9.
[0089] Comparative Example 4
[0090] The same as Example 1, except that the mass percentage of each component is:
[0091]
[0092] The balance was deionized water.
[0093] Comparative Example 5
[0094] The same as Example 1, except that the mass percentage of each component is:
[0095]
[0096]
[0097] The balance was deionized water.
[0098] Comparative Example 6
[0099] Commercially used carbon fiber precursor oil J-OA.
[0100] Performance Testing
[0101] 1. Carbon fiber precursor oil property test: The carbon fiber precursor oils of Examples 1-6 and Comparative Examples 1-6 were tested for appearance, solid content, viscosity and epoxy value in the following manner:
[0102] Appearance test: visual inspection;
[0103] Solid content test: carried out in accordance with national standard GB / T 2793-1995;
[0104] Viscosity test: carried out in accordance with national standard GB / T 2794-2013;
[0105] Epoxy value test: carried out in accordance with national standard GB / T 4612-2018.
[0106] The results are as follows:
[0107] Appearance Solid content (%) Viscosity (mPa·S) Epoxy value (eq / 100g) Example 1 White emulsion 31.19 160 0.19 Example 2 White emulsion 29.21 133 0.16 Example 3 White emulsion 30.51 157 0.18 Example 4 White emulsion 32.42 171 0.21 Example 5 White emulsion 29.87 155 0.17 Example 6 White emulsion 30.88 165 0.19 Comparative Example 1 White emulsion 28.46 130 0.16 Comparative Example 2 Translucent emulsion 27.52 110 0.14 Comparative Example 3 White emulsion 26.93 114 0.11 Comparative Example 4 White emulsion 27.41 165 0.12 Comparative Example 5 Clear transparent liquid 29.54 128 0.17 Comparative Example 6 Clear transparent liquid 26.54 101 0.11
[0108] According to the performance comparison of the carbon fiber precursor oil of Examples 1-6 and Comparative Example 6, it can be seen that the carbon fiber precursor oil provided by the present invention has a higher solid content, viscosity and epoxy value.
[0109] According to the performance comparison of the carbon fiber precursor oil of Examples 1-6 and Comparative Examples 1-2, it can be seen that the modified siloxane used in the present invention can effectively improve the viscosity and epoxy value of the carbon fiber precursor oil, and can enhance its adhesion ability to polyacrylonitrile fiber.
[0110] According to the performance comparison of the carbon fiber precursor oil of Examples 1-6 and Comparative Example 3, the present invention can effectively improve the epoxy value of the precursor oil by mixing fatty alcohol polyoxyethylene ether and fatty acid polyoxyethylene ester, and further modifying the modified siloxane after a part of them undergoes epoxycyclopropane reaction; and a part of them is used in a compound manner to enhance the adhesion ability of the precursor oil to polyacrylonitrile fiber.
[0111] According to the performance comparison of the carbon fiber precursor oil of Examples 1-6 and Comparative Examples 4-5, it can be seen that the component ratio of the carbon fiber precursor oil provided by the present invention can maximize the performance of the precursor oil, and too low or too high content of each component will affect its solid content, viscosity and epoxy value.
[0112] The carbon fiber precursor oils of Examples 1-6 and Comparative Examples 1-6 were used to oil the precursors, and then the T300 carbon fibers were processed, and finally the formed carbon fibers were measured.
[0113] 2. Determine the broken yarn, wool yarn, number of strands, oiling rate and fineness of the raw yarn during the pre-oxidation process as follows:
[0114] Determine the broken silk and wool in the pre-oxidation process: Observe whether there are broken silk and wool in the pre-oxidation process;
[0115] Determination of the number of parallel threads during pre-oxidation: Cut the fiber bundle into 3 mm lengths, disperse it in acetone, stir it for 10 minutes, and then disperse it on filter paper. Count the number of parallel threads between the monofilaments under a magnifying glass. Evaluate according to the following standards: A: less than 5, B: 5-10, C: more than 10;
[0116] Elastic composite fiber fineness test: in accordance with national standard GB / T 14343-2008;
[0117] The results are as follows:
[0118]
[0119]
[0120] According to the performance comparison of the carbon fiber precursor oil agent of Examples 1-6 and Comparative Example 6, it can be seen that during the pre-oxidation process of the carbon fiber precursor oil agent provided by the present invention, the precursor has no broken fibers or woolen threads, and the number of parallel strands of the precursor can be greatly reduced. The fineness of the obtained precursor is also lower than that of existing products, and it has a very high oiling rate.
[0121] According to the comparison of the performance of the raw silk in the pre-oxidation process of Examples 1-6 and Comparative Examples 1-2, the modified siloxane used in the present invention has strong compatibility with water, and a stable emulsion can be prepared after mechanical emulsification, which can reduce the number of raw silk breakage, wool and parallel yarns in the pre-oxidation process, has a high ammonia value, and a high oiling rate. It can be uniformly and strongly attached to polyacrylonitrile fibers, and the obtained raw silk has a very small fineness.
[0122] According to the comparison of the performance of the raw silk during the pre-oxidation process of Examples 1-6 and Comparative Example 3, it can be seen that the present invention can further modify the modified siloxane by mixing fatty alcohol polyoxyethylene ether and fatty acid polyoxyethylene ester, thereby enhancing the adhesion ability and uniformity of the raw silk oil agent to the polyacrylonitrile fiber; fatty alcohol polyoxyethylene ether and fatty acid polyoxyethylene ester are compounded to further enhance their oiling rate and oiling uniformity.
[0123] According to the comparison of the performance of the precursor during the pre-oxidation process of Examples 1-6 and Comparative Examples 4-5, it can be seen that the component ratio of the carbon fiber precursor oil provided by the present invention can maximize the performance of the precursor oil. Too low or too high a content of each component will affect the breakage, wool and parallel yarn number of the precursor, and affect the oil application rate of the oil and the fineness of the precursor.
[0124] 3. The linear density and bundle strength of the carbon fibers prepared from the carbon fiber precursor oils of Examples 1-6 and Comparative Examples 1-6 were tested as follows:
[0125] Linear density test: carried out in accordance with national standard GB / T 16256-1996;
[0126] Bundle strength test: carried out in accordance with standard GB / T 14344-2008.
[0127] The results are as follows:
[0128]
[0129]
[0130] According to the performance comparison of the carbon fiber precursor oil agent of Examples 1-6 and Comparative Example 6, it can be known that the carbon fiber precursor oil agent provided by the present invention can effectively improve the internal structural defects and loose core of the carbon fiber precursor produced in the pre-oxidation stage, and the problem of large holes; and the oiling process has a better oiling rate and oiling uniformity for polyacrylonitrile fiber, so that the prepared carbon fiber has a higher linear density and bundle strength.
[0131] According to the comparison of the carbon fiber performance of Examples 1-6 and Comparative Examples 1-2, it can be seen that the modified siloxane used in the present invention can form a stable emulsion and has a higher ammonia value, so that the carbon fiber obtained has a higher and more uniform oiling rate, and therefore has a higher linear density and bundle strength.
[0132] According to the comparison of the carbon fiber performance of Examples 1-6 and Comparative Example 3, the present invention further modifies the modified siloxane by mixing fatty alcohol polyoxyethylene ether and fatty acid polyoxyethylene ester to produce an epoxy cyclopropane addition reaction, so that the epoxy group and the carboxyl group are linked and the hydrophilic polyether chain segment is grafted to make the modified silicone oil have stronger water solubility and dispersibility, and the prepared raw silk oil agent is more uniform and stable, and its adhesion ability to polyacrylonitrile fiber is enhanced; by compounding fatty alcohol polyoxyethylene ether and fatty acid polyoxyethylene ester, the overall dispersibility and water solubility of the raw silk oil agent are enhanced, and its oiling rate and oiling uniformity are further enhanced.
[0133] According to the comparison of the carbon fiber performance of Examples 1-6 and Comparative Examples 4-5, it can be seen that the component ratio of the carbon fiber precursor oil provided by the present invention can maximize the performance of the precursor oil, and too low or too high content of each component will affect the linear density and bundle strength of the obtained carbon fiber.
[0134] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A carbon fiber precursor oil, characterized in that: Containing modified siloxane, fatty alcohol polyoxyethylene ether, nonionic antistatic agent, fatty acid polyoxyethylene ester, antioxidant and deionized water; The modified siloxane is a compound of formula I: , Where m=5-10, n=50-60; The preparation method of the modified siloxane is as follows: under nitrogen protection, cyclosiloxane, aminosilane, catalyst and end-capping agent are mixed, gradually heated to 150-160° C., reacted for 20-24 hours, then heated to 180-185° C., reacted for 3-5 minutes, then cooled and filtered to obtain the modified siloxane; The carbon fiber precursor oil is prepared by the following steps: (1) Add fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester, nonionic antistatic agent and antioxidant into a stirring kettle, stir at 50-55°C for 1-2 hours to obtain a uniform composite emulsion for use; (2) slowly adding the modified siloxane into a high shear emulsifier, starting the stirring, slowly adding the pre-prepared composite emulsifier into the emulsifier, adjusting the temperature at 40-50°C, and after all the composite emulsifiers are added, adding deionized water dropwise thereto, adjusting the pH to 4.5-5.5, controlling the stirring speed to 2800-3200 r / min, stirring for 100-140 minutes, stirring evenly, cooling to room temperature, and filtering to obtain a white emulsion, which is the carbon fiber precursor oil agent; The general formula of the fatty alcohol polyoxyethylene ether in step (1) is RO(CH2CH2O)xH, wherein x=10-20, and R is a straight-chain or branched saturated alkane with 12-18 carbon atoms; the structural formula of the fatty acid polyoxyethylene ester is RCOO(EO)yH, wherein y=3-40, and R is a straight-chain or branched hydrocarbon with 4-20 carbon atoms; In step (1), the nonionic antistatic agent is selected from one of glycerol stearate, fatty acid polyol ester or ethanolamide; In the step (1), the antioxidant is selected from one or a mixture of antioxidant 1076, antioxidant 1035 or phenolic antioxidant BHT.
2. The carbon fiber precursor oil according to claim 1, characterized in that Taking the total mass as 100%, the mass percentage of each component is: Modified siloxane 40-55% Fatty alcohol polyoxyethylene ether 10-20% Nonionic antistatic agent 10-15% Fatty acid polyoxyethylene ester 10-20% Antioxidant 1-3% The balance was deionized water.
3. The carbon fiber precursor oil according to claim 1, characterized in that The cyclosiloxane is selected from hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane or dodecamethylcyclohexasiloxane; and the aminosilane is N-aminoethyl-3-aminopropylmethyldimethoxysilane.
4. The carbon fiber precursor oil according to claim 1, characterized in that The catalyst is selected from one of sodium hydroxide, potassium hydroxide, sodium methoxide, tetramethylammonium hydroxide or tetramethylguanidine; and the end-capping agent is hexamethyldisiloxane.
5. The carbon fiber precursor oil according to claim 1, characterized in that: The mass ratio of the cyclosiloxane, aminosilane and end-capping agent is (25-35):(1-5):(0.5-1).