A preparation method and product of dopamine electrochemical sensor

By using bimetallic MOF-derived magnetic NiO-Co3O4@CNTs/rGO modification technology on electrochemical sensors, the problems of poor conductivity and few active sites of dopamine electrochemical sensors are solved, and efficient and sensitive dopamine detection is achieved, with low detection Outsourcing and good stability and anti-interference ability.

CN115791941BActive Publication Date: 2024-11-19XIANGTAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211110794.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-13
Publication Date
2024-11-19
Estimated Expiration
2042-09-13

AI Technical Summary

Technical Problem

Existing dopamine electrochemical sensors have problems such as poor conductivity and low exposure of active sites, which leads to poor oxidation electrical signal of dopamine and low efficiency.

Method used

The preparation method of electrochemical sensors modified by bimetallic MOF derived magnetic NiO-Co3O4@CNTs/rGO is used to prepare an electrochemical sensor. Through ultrasonic dispersion and electrodeposition technology, NiO-Co3O4@CNTs are deposited on the surface of glass carbon electrodes, and the activity is formed by scanning by cyclic voltammetry. Electrocatalytic surface with many sites.

Benefits of technology

It has achieved a lower detection limit, a wide detection range, outstanding selectivity and stability, and has significantly improved the detection effect of dopamine, can effectively resist interfering substances, and has good reproducibility and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115791941B_ABST
    Figure CN115791941B_ABST
Patent Text Reader

Abstract

The present application relates to a preparation method and product of a dopamine electrochemical sensor. NiCo‑TPA is synthesized by a traditional hydrothermal method and then pyrolyzed to obtain NiO‑Co3O4@CNTs. Subsequently, NiO‑Co3O4@CNTs / rGO / GCE electrochemical sensor is prepared by electrodeposition on the surface of reduced graphene oxide, with the help of the excellent electron conductivity of rGO and the active sites of NiCo@CNTs. The sensor has a lower detection limit, a wide detection range, and excellent selectivity and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electrochemical detection, and specifically relates to a method for preparing a bimetallic MOF-derived magnetic NiO-Co3O4@CNTs / rGO-modified dopamine electrochemical sensor. Background Art

[0002] Neurotransmitters are a very critical chemical signal transmission in the human body. They connect various organs, nerves and muscle cells of the human body, promote the normal functioning of the human body, and play a very important role in regulating the functions of various organs. Dopamine is one of the most important neurotransmitters. Many studies have shown that dopamine plays an important role in many physiological systems of the human body. Other studies have shown that dopamine is also related to addiction. Some drugs can cause addiction by controlling the secretion of dopamine in the brain. Dopamine is an important sign of human health, and its indicators are the key to the diagnosis and treatment of dopamine dysfunction in clinical practice. Therefore, research and development are of great practical significance for in vivo and in vitro dopamine detection. In recent years, a variety of detection methods for dopamine content in human serum and urine have been studied and developed. For example, spectrophotometry, high performance liquid chromatography and other methods have been applied to in vitro detection of dopamine.

[0003] However, the above methods are expensive, take a long time to measure, and require professional technicians to measure, which is inefficient. At this time, efficient, sensitive and low-cost electrochemical sensors have entered the field of vision of researchers. Electrochemical sensors mainly rely on electrocatalytic materials modified on the surface of electrodes. The two ortho-phenolic hydroxyl groups of dopamine provide the electrochemical activity of its molecules, and then through the catalytic oxidation of the electrode surface material, a strong electrical signal can be formed. However, electrode surface materials generally have the disadvantages of poor conductivity and less exposure of active sites, which to a certain extent prevent the oxidation electrical signal of dopamine. Summary of the invention

[0004] The technical problem to be solved by the present invention is: to solve the deficiencies in the prior art, thereby providing a preparation method and product of a dopamine electrochemical sensor with more exposed active sites and high electrocatalytic activity.

[0005] The technical solution adopted by the present invention to solve its technical problem is:

[0006] A method for preparing a dopamine electrochemical sensor comprises the following steps:

[0007] S1: Take terephthalic acid, polyvinyl pyrrolidone, nickel nitrate and cobalt nitrate, and then dissolve them in a mixed solution of deionized water, DMF and ethanol, and ultrasonically disperse them for more than half an hour to ensure that they are completely dissolved. After the solution is clear, transfer it to a reactor and place it in an oven for reaction. After the reaction is completed and naturally cooled, centrifuge it using a high-speed centrifuge and wash it with DMF, methanol and water in turn, and finally dry it in a vacuum to obtain NiCo-MOF; anneal the prepared NiCo-MOF in a tubular furnace to obtain a magnetic black powder, namely NiO-Co3O4@CNTs. Weigh the NiO-Co3O4@CNTs powder and add it to the DMF solution, then add NaCl, and ultrasonically disperse the suspension to obtain a NiO-Co3O4@CNTs electrodeposition solution;

[0008] Taking a polished and dried glassy carbon electrode and inserting it into a graphite oxide electrodeposition solution, scanning the glassy carbon electrode by cyclic voltammetry and then drying it to obtain a glassy carbon electrode after graphite oxide deposition;

[0009] S2: The NiO-Co3O4@CNTs electrodeposition solution is electrodeposited onto the graphite oxide of the glassy carbon electrode by cyclic voltammetry scanning and the graphene oxide on the glassy carbon electrode is reduced;

[0010] S3: placing the glassy carbon electrode obtained in step S2 in a blank PBS buffer solution, and then performing cyclic voltammetry scanning to reduce graphite oxide to obtain a dopamine electrochemical sensor.

[0011] Preferably, in the preparation method of the dopamine electrochemical sensor of the present invention, in step S2, cyclic voltammetry is used to measure the potential in the range of -0.2V to 1.2V at 0.1V·s- 1 The graphene oxide was scanned at a speed of 20 and a half circles, and stirring was maintained during the scanning. After the scanning, it was placed under an infrared lamp to dry. NiO-Co3O4@CNTs was then electrodeposited on the graphene oxide, and cyclic voltammetry was used at 0.1V·s -1 The scanning rate was scanned for 5 cycles in the potential range of -1.2V to 2.0V to allow graphene oxide to be electrodeposited on the electrode surface. The electrode was then taken out and dried under an infrared lamp. The obtained electrode was placed in a blank 0.1M PBS buffer solution with a pH of 5.5. Cyclic voltammetry was used to scan in the potential range of -0.9V to 0V at a scanning rate of 0.1V·s-1 to reduce graphene oxide. Finally, the NiCo@CNTs / rGO / GCE electrochemical sensing platform was successfully prepared.

[0012] Preferably, in the preparation method of the dopamine electrochemical sensor of the present invention, before step S1, the glassy carbon electrode is first treated, and the glassy carbon electrode is first polished using alumina powders with particle sizes of 1.0um, 0.3um, and 0.05um in sequence, and then the polished electrode is immersed in anhydrous ethanol and deionized water in sequence for ultrasonic washing. In step S1, the volume ratio of the mixed solution of deionized water, DMF and ethanol is 1:1:1.

[0013] Preferably, in the method for preparing the dopamine electrochemical sensor of the present invention, the oven temperature in step S1 is 150° C. and the reaction time is 10 h.

[0014] Preferably, in the method for preparing the dopamine electrochemical sensor of the present invention, the annealing temperature of the tube furnace in step S1 is 400°C, and the heating rate is 2°C·min -1 , annealing time is 4h, and the NaCl concentration in step S1 is 15mmol·L -1 .

[0015] Preferably, in the method for preparing the dopamine electrochemical sensor of the present invention, the concentration of the NiO-Co3O4@CNTs electrodeposition solution in step S1 is 2 mg·mL -1 .

[0016] Preferably, in the preparation method of the dopamine electrochemical sensor of the present invention, the synthesis method of graphene oxide in step S2 includes: first taking graphite powder and mixing it with sodium nitrate and slowly adding it to cold concentrated H2SO4, stirring the solution in an ice water bath and keeping the overall temperature of the reaction below 5°C, slowly adding KMnO4 during the stirring reaction, removing the ice bath device, and then reacting at room temperature with continuous stirring, then adding deionized water to the reaction solution, and at the same time raising the reaction temperature to 80-120°C, then adding deionized water and hydrogen peroxide solution to the reaction until the reaction stops and the solution is light brown, leaving it and filtering it to obtain a brown precipitate, then repeatedly washing it with dilute hydrochloric acid, and finally, centrifuging it with deionized water, drying it in a vacuum drying oven, collecting graphene oxide, weighing the graphene oxide powder, adding it to deionized water, and then adding NaCl as a supporting electrolyte, and ultrasonically mixing the dispersion at room temperature to obtain a graphene oxide electrodeposition solution.

[0017] Preferably, in the method for preparing a dopamine electrochemical sensor of the present invention, the mass fraction of hydrogen peroxide in step S2 is 30%, and the dilute hydrochloric acid is prepared from a concentrated hydrochloric acid solution and water in a volume ratio of 5:95, wherein the mass fraction of the concentrated hydrochloric acid solution is 36%-38%.

[0018] Preferably, in the method for preparing the dopamine electrochemical sensor of the present invention, the concentration of NaCl in step S2 is 5 mmol·L -1The concentration of graphite oxide electrodeposition solution in step S2 is 2 mg mL -1 .

[0019] Preferably, the method for preparing the dopamine electrochemical sensor of the present invention uses cyclic voltammetry at a potential range of -0.2V to 1.2V at 0.1V·s- 1 The graphene oxide was scanned at a speed of 20 and a half circles, and stirring was maintained during the scanning. After the scanning, it was placed under an infrared lamp to dry. NiO-Co3O4@CNTs was then electrodeposited on the graphene oxide, and cyclic voltammetry was used at 0.1V·s -1 The scanning rate was scanned for 5 cycles in the potential range of -1.2V to 2.0V to allow graphene oxide to be electrodeposited on the electrode surface. The electrode was then taken out and dried under an infrared lamp. Finally, the graphene oxide on the electrode was reduced. The obtained electrode was placed in a blank 0.1M PBS buffer solution with a pH of 5.5. Cyclic voltammetry was used to scan in the potential range of -0.9V to 0V at a scanning rate of 0.1V·s-1 to reduce the graphene oxide. Finally, the NiCo@CNTs / rGO / GCE electrochemical sensing platform was successfully prepared.

[0020] The present invention also provides a dopamine electrochemical sensor, which is prepared by the above-mentioned preparation method.

[0021] The beneficial effects of the present invention are:

[0022] The present invention synthesizes NiCo-TPA by a traditional hydrothermal method, and then pyrolyzes it to obtain NiO-Co3O4@CNTs, which is then electrodeposited on the surface of reduced graphene oxide. By virtue of the excellent electronic conductivity of rGO and the active sites of NiCo@CNTs, a NiO-Co3O4@CNTs / rGO / GCE electrochemical sensor is prepared, which has a lower detection limit, a wide detection range, and outstanding selectivity and stability.

[0023] The present invention combines the advantages of NiO-Co3O4@CNTs such as large specific surface area, multiple active sites, excellent conductivity and surface active groups of reduced graphene oxide, so that the detection effect of dopamine is greatly increased. After optimizing the experimental conditions and measuring the working curve of dopamine by differential pulse voltammetry, the following experimental conclusions are obtained: when the dopamine concentration is 100nM-7μM and 7μM-22μM, it presents two linear segments, and the linear equations are, respectively, Ip1(μA)=0.0064C(nM)-0.6783(R 2 =0.9975), Ip2(μA)=0.0013C(nM)+33.787(R 2=0.9916) with a detection limit (LOD) of 45nM (S / N=3), and the sensor prepared in this way also has a good resistance to interferences in the solution to be tested. In addition, the sensor also has good reproducibility and stability, and has been successfully used to detect dopamine in actual samples. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The technical solution of the present application is further described below in conjunction with the accompanying drawings and embodiments.

[0025] Figure 1A is the SEM image of NiCo-TPA-MOF in Example 1, Figure 1B This is the SEM image of NiO-Co3O4@CNTs / rGO in Example 1.

[0026] Figure 2A This is the DPV spectrum of NiO-Co3O4@CNTs / rGO / GCE to different concentrations of dopamine in Example 1. Figure 2B This is the working curve of NiO-Co3O4@CNTs / rGO / GCE for dopamine detection in Example 1.

[0027] Figure 3 For Example 1, the effect of interferon on 5 μM dopamine was tested. DETAILED DESCRIPTION

[0028] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application may be combined with each other.

[0029] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the scope of protection of the present application. In addition, the terms "first", "second", etc. are used only for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the invention, unless otherwise specified, "multiple" means two or more.

[0030] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood by specific circumstances.

[0031] The technical solution of the present application will be described in detail below with reference to the accompanying drawings and in combination with embodiments.

[0032] Example 1

[0033] This embodiment provides a method for preparing a dopamine electrochemical sensor, comprising the following steps:

[0034] S1: Preparation of NiO-Co3O4@CNTs electrodeposition solution: 0.15g terephthalic acid (TPA), 1.5g polyvinyl pyrrolidone (PVP), 0.067g nickel nitrate and 0.132g cobalt nitrate were taken, and then dissolved in a deionized water:DMF:ethanol solution with a volume ratio of 1:1:1, and ultrasonically dispersed for more than 40 minutes to ensure complete dissolution. After the solution became clear, it was transferred to a reactor and placed in an oven at 150°C for 10 hours. After complete cooling, it was centrifuged at 12000rpm for 5 minutes using a high-speed centrifuge and washed with DMF, methanol and water in turn. Finally, it was vacuum dried at 70°C for 12 hours to obtain NiCo-MOF. The prepared NiCo-MOF was placed in a tubular furnace and heated to 400°C (according to 2°C·min -1 The heating rate was increased) and maintained for 3 h, and finally a black powder with magnetic properties was obtained, namely NiO-Co3O4@CNTs. 20 mg of NiO-Co3O4@CNTs powder was weighed and added to 10 mL of DMF solution, and then 15 mmol of NaCl was added, and the suspension was ultrasonically dispersed for 2 h to obtain 2 mg·mL-1 NiO-Co3O4@CNTs electrodeposition solution.

[0035] S2: Synthesis of graphene oxide (GO), first take 6g of graphite powder and mix it with 3g of sodium nitrate and slowly add it to cold concentrated H2SO4, stir the solution in an ice water bath and keep the overall temperature of the reaction below 5°C. In the stirring reaction, slowly add 15g of KMnO4, remove the ice bath device, and then react at room temperature with continuous stirring. Then add 200mL of deionized water to the reaction solution, and raise the reaction temperature to 98°C, then add 500mL of deionized water and 30mL of 30% hydrogen peroxide solution to the reaction until the reaction stops and the solution is light brown, leave it overnight, filter it to get a brown precipitate, and then wash it repeatedly with dilute hydrochloric acid (dilute hydrochloric acid is composed of a concentrated hydrochloric acid solution and water with a volume ratio of 5:95, and the mass fraction of the concentrated hydrochloric acid solution is 36%-38%.). Finally, centrifuge with deionized water, dry it in a vacuum drying oven, and collect graphene oxide. 10 mg of graphene oxide powder was weighed and added to 10 mL of deionized water. 5 mmol of NaCl was added as a supporting electrolyte. The dispersion was ultrasonically mixed at 25 °C for 6 h to obtain 2 mg mL -1 GO electrodeposition solution.

[0036] S3: Construction of NiO-Co3O4@CNTs / rGO / GCE electrochemical sensing platform: Before using the glassy carbon electrode for testing experiments, it should be polished with alumina powders with particle sizes of 1.0um, 0.3um, and 0.05um in sequence, and then the polished electrode should be immersed in anhydrous ethanol and deionized water for ultrasonic cleaning in sequence. After washing, the clean electrode should be placed under an infrared lamp for drying. First, graphene oxide is attached to the surface of the electrode, and the operation is carried out according to the description in the literature. The prepared electrode is first inserted into the electrodeposition solution of GO, and the cyclic voltammetry method is used to conduct the ultrasonic cleaning at a potential range of -0.2V to 1.2V at 0.1V·s -1 The graphene oxide was scanned at a speed of 20 half circles, with stirring during the process. After the scanning, it was placed under an infrared lamp to dry. NiCo@CNTs was then electrodeposited on the graphene oxide, and CV was used at 0.1 V·s -1 The scanning rate was scanned for 5 cycles in the potential range of -1.2V to 2.0V to allow graphene oxide to be electrodeposited on the electrode surface. The electrode was then taken out and dried under an infrared lamp. Finally, the graphene oxide on the electrode was reduced. According to the description in the literature, the obtained electrode was placed in a blank 0.1M pH=5.5 PBS buffer solution, and the CV technology was used to scan at a scanning rate of 0.1V·s-1 in the potential range of -0.9V to 0V to reduce GO to generate rGO (reduced graphite oxide). Finally, the NiO-Co3O4@CNTs / rGO / GCE electrochemical sensing platform was successfully prepared.

[0037] Effect Example

[0038] Take the Co3O4 / N-CNFs / MoS2-MWCNTs / GCE electrochemical sensor prepared in Example 1 as an example, and use it to detect the concentration of dopamine. As shown in Figure 2a, by adding luteolin of different concentrations (100nM~7μM and 7μM~22μM), the differential pulse voltammetry (DPV) of the Co3O4 / N-CNFs / MoS2-MWCNTs / GCE electrochemical sensor in response to luteolin can be obtained. Figure 2b is the calibration curve of the response current and concentration of luteolin. It can be seen that when the dopamine concentration is 100nM~7μM and 7μM~22μM, it is linear in two sections, and the linear equations are, Ip1(μA)=0.0064C(nM)-0.6783(R 2 =0.9975), Ip2(μA)=0.0013C(nM)+33.787(R 2 =0.9916), and the limit of detection (LOD) was 45nM (S / N=3).

[0039] Taking the prepared NiO-Co3O4@CNTs / rGO / GCE electrochemical sensor as an example, the effect of interferon on 5μM dopamine was tested. Figure 3 As shown, when different interferents were added to measure the performance of the sensor for dopamine detection, the peak current value hardly decreased, indicating that the prepared NiO-Co3O4@CNTs / rGO / GCE electrochemical sensor has good anti-interference ability.

[0040] Bimetallic MOF: NiCo-MOF, and after carbonization at 400 ° C, it was electrodeposited on reduced graphene oxide, thereby constructing a new dopamine electrochemical sensing platform NiO-Co3O4@CNTs / rGO / GCE. This electrode material combines the advantages of NiO-Co3O4@CNTs, such as large specific surface area and multiple active sites, and reduced graphene oxide, such as excellent conductivity and surface active groups, which greatly increases its detection effect on dopamine. After optimizing the experimental conditions and using differential pulse voltammetry to determine the working curve of dopamine, the following experimental conclusions were drawn: When the dopamine concentration is 100nM~7μM and 7μM~22μM, it presents two linear segments, and the linear equations are, Ip1(μA)=0.0064C(nM)-0.6783(R 2 =0.9975), Ip2(μA)=0.0013C(nM)+33.787(R 2 =0.9916), the detection limit (LOD) is 45nM (S / N=3), and the sensor prepared in this way also has a good resistance to interferences in the solution to be tested. In addition, the sensor also has good reproducibility and stability, and has been successfully used to detect dopamine in actual samples.

[0041] Based on the above ideal embodiments of this application, the relevant staff can make various changes and modifications without departing from the technical concept of this application through the above description. The technical scope of this application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a dopamine electrochemical sensor, characterized in that: The detection range is 100nM~22μM and includes the following steps: S1: Take terephthalic acid, polyvinyl pyrrolidone, nickel nitrate and cobalt nitrate, and then dissolve them in a mixed solution of deionized water, DMF and ethanol, and ultrasonically disperse them for more than half an hour to ensure that they are completely dissolved. After the solution is clear, transfer it to a reactor and place it in an oven for reaction. After the reaction is completed and naturally cooled, use a high-speed centrifuge to centrifuge and wash with DMF, methanol and water in turn, and finally vacuum dry to obtain NiCo-MOF; place the prepared NiCo-MOF in a tubular furnace for annealing to obtain a magnetic black powder, namely NiO-Co3O4@CNTs, weigh the NiO-Co3O4@CNTs powder and add it to the DMF solution, then add NaCl, and ultrasonically disperse the suspension to obtain a NiO-Co3O4@CNTs electrodeposition solution; Taking a polished and dried glassy carbon electrode and inserting it into a graphite oxide electrodeposition solution, scanning the glassy carbon electrode by cyclic voltammetry and then drying it to obtain a glassy carbon electrode after graphite oxide deposition; S2: The NiO-Co3O4@CNTs electrodeposition solution is electro-deposited onto the graphite oxide of the glassy carbon electrode by cyclic voltammetry scanning to obtain graphene oxide; S3: placing the glassy carbon electrode obtained in step S2 in a blank PBS buffer solution, and then performing cyclic voltammetry scanning to reduce graphite oxide to obtain a dopamine electrochemical sensor; The annealing temperature of the tube furnace in step S1 is 400°C, and the heating rate is 2°C·min -1 , annealing time is 4h, and the NaCl concentration in step S1 is 15mmol·L -1 ; The concentration of NiO-Co3O4@CNTs electrodeposition solution in step S1 is 2 mg mL -1 ; The synthesis method of graphene oxide in step S2 includes: first taking graphite powder and mixing it with sodium nitrate and slowly adding it to cold concentrated H2SO4, stirring the solution in an ice water bath and keeping the overall temperature of the reaction below 5°C, slowly adding KMnO4 during the stirring reaction, removing the ice bath device, continuing the reaction at room temperature, and continuously stirring, then adding deionized water to the reaction solution, and at the same time raising the reaction temperature to 80-120°C, then adding deionized water and hydrogen peroxide solution to the reaction until the reaction stops and the solution turns light brown, leaving it and filtering it to obtain a brown precipitate, then repeatedly washing it with dilute hydrochloric acid, and finally centrifuging it with deionized water, drying it in a vacuum drying oven, collecting graphene oxide, weighing graphene oxide powder, adding it to deionized water, and then adding NaCl as a supporting electrolyte, placing the dispersion at room temperature for ultrasonic mixing to obtain a graphene oxide electrodeposition solution; In step S2, the mass fraction of hydrogen peroxide is 30%, and the dilute hydrochloric acid is prepared by a concentrated hydrochloric acid solution and water in a volume ratio of 5:95, wherein the mass fraction of the concentrated hydrochloric acid solution is 36%-38%; The NaCl concentration in step S2 is 5 mmol·L -1 The concentration of graphite oxide electrodeposition solution in step S2 is 2 mg mL -1 .

2. The method for preparing a dopamine electrochemical sensor according to claim 1, characterized in that: In step S2, cyclic voltammetry was used to measure the potential in the range of -0.2 V to 1.2 V at a rate of 0.1 V·s -1 The graphene oxide was scanned at a speed of 20 and a half circles, and stirring was maintained during the scanning. After the scanning, it was placed under an infrared lamp to dry. NiO-Co3O4@CNTs was then electrodeposited on the graphene oxide, and cyclic voltammetry was used at 0.1V·s -1 The scanning rate was scanned for 5 cycles in the potential range of -1.2V to 2.0V to allow graphene oxide to be electrodeposited on the electrode surface, and then the electrode was taken out and dried under an infrared lamp; In step S3, the obtained electrode was placed in a blank 0.1 M PBS buffer solution with a pH of 5.5 and a current of 0.1 V·s -1 The scan rate was scanned in the potential range of -0.9V to 0V using cyclic voltammetry to reduce graphite oxide, and finally the NiCo@CNTs / rGO / GCE electrochemical sensing platform was successfully prepared.

3. The method for preparing a dopamine electrochemical sensor according to claim 1, characterized in that: Before step S1, the glassy carbon electrode is first processed. The glassy carbon electrode is first polished with alumina powders with particle sizes of 1.0 μm, 0.3 μm, and 0.05 μm, respectively. The polished electrode is then immersed in anhydrous ethanol and deionized water for ultrasonic washing. The volume ratio of the mixed solution of deionized water, DMF, and ethanol in step S1 is 1:1:

1.

4. The method for preparing a dopamine electrochemical sensor according to claim 1, characterized in that: In step S1, the oven temperature is 150° C. and the reaction time is 10 h.

5. A dopamine electrochemical sensor, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 4.