A catalyst for preparing hydroxyaromatic ketone and its preparation method and application

By using an organometallic skeleton material and a catalyst of benzyl functionalized ionic liquid, the problems of low conversion of phenolic ester and selectivity of hydroxyarosterone in the prior art are solved, and more efficient hydroxyarosterone synthesis is achieved.

CN115805101BActive Publication Date: 2024-11-29CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111067853.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-13
Publication Date
2024-11-29
Estimated Expiration
2041-09-13

AI Technical Summary

Technical Problem

In the catalytic synthesis of hydroxyarones by substituted alkylphenol esters or halogenated phenol esters, the phenol ester conversion and hydroxyarone selectivity are low.

Method used

The performance of the catalyst is improved by confining the benzyl-functionalized ionic liquid in situ in the pore of MIL-101 (Cr) using a catalyst including an organometallic skeleton material and a benzyl-functionalized ionic liquid.

Benefits of technology

The conversion of phenolic ester and the selectivity of hydroxyarone are significantly improved, and the efficiency of the catalyst is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115805101B_ABST
    Figure CN115805101B_ABST
Patent Text Reader

Abstract

The present invention relates to a catalyst for preparing hydroxyaromatic ketone, a preparation method thereof and an application thereof. The catalyst comprises an organic metal framework material and a benzyl-functionalized ionic liquid; and the catalyst has a unique X-ray diffraction pattern. The benzyl-functionalized ionic liquid in the catalyst of the present invention is in-situ confined in the pores of the organic metal framework material, thereby improving the performance of the benzyl-functionalized ionic liquid. The catalyst prepared by the method of the present invention is applied to the preparation of hydroxyaromatic ketone, which has the characteristics of improving the conversion rate of phenolic ester and the selectivity of hydroxyaromatic ketone.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation of hydroxyaromatic ketones, and particularly relates to a catalyst for preparing hydroxyaromatic ketones, a preparation method and application thereof. Background Art

[0002] Hydroxyaromatic ketone molecules contain hydroxyl and ketone groups on the benzene ring. They are very important fine chemicals and synthetic intermediates, and are widely used in the fields of medicine, cosmetics, food, synthetic materials, etc. Among them, p-hydroxyacetophenone is an example. It is a natural plant extract that naturally exists in the stems and leaves of the Asteraceae plant Artemisia scoparia, the roots of Artemisia capillaris, Asclepiadaceae plants, and Panax ginseng. It has important application value in the fields of medicine, dyes, cosmetics, liquid crystal materials, synthetic resins, etc. Ortho-hydroxyacetophenone is mainly used as a pharmaceutical intermediate and fragrance, such as an important intermediate of the IA class antiarrhythmic drug propafenone hydrochloride and the antifungal drug croconazole hydrochloride.

[0003] The main methods for synthesizing hydroxyacetophenone include phenyl acetate method, p-aminoacetophenone method, photocatalysis method, etc. Among them, the phenyl acetate method is to obtain hydroxyacetophenone by intramolecular rearrangement of phenyl acetate, which has a high atomic utilization rate and is therefore very popular. Its effective catalytic system is Lewis acid, Acid and ionic liquid catalysts, however, have the disadvantage of low selectivity for para-hydroxyaryl ketones.

[0004] Metal organic framework materials are a class of polymer crystal materials with intrinsic amphiphilic structures. The polar nodes in the MOFs structure can strongly interact with molecules through various forces such as coordination, ion exchange, and electrostatic effects; and MOFs have rich pore structure characteristics, which is conducive to the preparation of composite materials through various methods such as in-situ embedding and post-modification to improve their application performance. Summary of the invention

[0005] The present invention aims at the problem of low phenol ester conversion rate and low hydroxy aromatic ketone selectivity in the prior art of catalyzing the synthesis of hydroxy aromatic ketone by substituted alkyl phenol ester or halogenated phenol ester, and provides a new catalyst for preparing hydroxy aromatic ketone. The catalyst has the characteristics of improving phenol ester conversion rate and hydroxy aromatic ketone selectivity.

[0006] To this end, the first aspect of the present invention provides a catalyst for preparing a hydroxyaromatic ketone, which comprises an organic metal framework material and a benzyl-functionalized ionic liquid; and the catalyst has an X-ray diffraction pattern substantially as follows;

[0007]

[0008] Wherein, (a) = ±0.3°.

[0009] The content of the organometallic framework material and the benzyl-functionalized ionic liquid in the catalyst of the present invention is the actual amount of the organometallic framework material and the benzyl-functionalized ionic liquid used in the synthesis of the catalyst. Since the benzyl-functionalized ionic liquid in the catalyst is confined in the pores of the organometallic framework material, the excess benzyl-functionalized ionic liquid that has not reacted in the pores will be washed away by the solvent. Therefore, the present invention does not clearly define the content of the organometallic framework material and the benzyl-functionalized ionic liquid in the catalyst, and those skilled in the art can adjust it according to actual needs.

[0010] In some embodiments of the present invention, the organic metal framework material is selected from one or more of IRMOF, ZIFs, PCPs and MIL, preferably MIL.

[0011] In the present invention, PCPs (porous coordination polymers) are a class of highly crystalline porous hybrid materials that connect metal clusters (or ions) and organic ligands through coordination bonds.

[0012] In some preferred embodiments of the present invention, the MIL is selected from one or more of MIL-53, MIL-100 and MIL-101, preferably MIL-101, and more preferably MIL-101(Cr).

[0013] In some embodiments of the present invention, the structure of the benzyl-functionalized ionic liquid contains cations formed by nitrogen heterocyclic organic compounds and benzyl halide compounds and metal halide.

[0014] In some embodiments of the present invention, the nitrogen heterocyclic organic compound is selected from one or more of imidazole, alkyl imidazole, pyridine, alkyl pyridine, pyrimidine, alkyl pyrimidine, pyrrole and alkyl pyrrole; preferably, the alkyl group is selected from at least one of the C1 to C5 alkyl groups; further preferably, the nitrogen heterocyclic organic compound is selected from one or more of pyridine, 4-methylpyridine, 3-methylpyridine and 3, 5-dimethylpyridine.

[0015] The second aspect of the present invention provides a method for preparing the catalyst according to the first aspect of the present invention, comprising the following steps:

[0016] S1, mixing solvent A, an organic metal framework material, a nitrogen heterocyclic organic compound and a benzyl halide compound, reacting the mixture, and then cooling, filtering, washing and drying the mixture to obtain a solid product;

[0017] S2, mixing solvent B, the solid product and Lewis acid, and reacting the mixture, followed by cooling, filtering, washing and drying to obtain the catalyst.

[0018] In some embodiments of the present invention, the molar ratio of the nitrogen heterocyclic organic compound, the benzyl halide compound and the Lewis acid is (0.5-1.5):(0.5-1.5):(1.5-2.5); preferably (0.8-1.2):(0.8-1.2):(1.8-2.2); more preferably 1:1:2.

[0019] The present invention does not clearly limit the amount of the organic metal framework material in the above reaction, and those skilled in the art can adjust it according to actual needs.

[0020] In some embodiments of the present invention, the nitrogen heterocyclic organic compound is selected from one or more of imidazole, alkyl imidazole, pyridine, alkyl pyridine, pyrimidine, alkyl pyrimidine, pyrrole and alkyl pyrrole; preferably, the alkyl group is selected from at least one of the C1 to C5 alkyl groups; further preferably, the nitrogen heterocyclic organic compound is selected from one or more of pyridine, 4-methylpyridine, 3-methylpyridine and 3, 5-dimethylpyridine.

[0021] In other embodiments of the present invention, the benzyl halide compound is selected from one or more of benzyl chloride, 2,4,6-trimethylbenzyl chloride, p-trifluoromethylbenzyl chloride, benzyl bromide and 4-isopropylbenzyl bromide.

[0022] In some embodiments of the present invention, the Lewis acid is selected from one or more of aluminum chloride, aluminum bromide, ferric chloride, zinc chloride, boron trifluoride, gallium chloride, indium chloride, and cuprous chloride; preferably selected from one or more of aluminum chloride and ferric chloride.

[0023] In other embodiments of the present invention, the solvent A and the solvent B are each independently selected from any one of chlorobenzene, nitrobenzene, toluene, nitromethane, acetonitrile and dichloromethane.

[0024] The present invention does not clearly limit the amount of solvent A and solvent B. Generally, as long as they can dissolve the corresponding solute, they can be used. In some specific embodiments of the present invention, the amount of the above solvent is such that the concentration of the corresponding solute (the solute required to be dissolved by the solvent) is 0.001 mol / L to the saturated solubility.

[0025] In the present invention, the organic metal framework material may be pre-dried before use.

[0026] In some other embodiments of the present invention, in step S1, the reaction temperature is 0 to 100°C, preferably 30 to 40°C; and / or the reaction time is 2 to 72 hours, preferably 12 to 15 hours.

[0027] In some embodiments of the present invention, in step S2, the reaction temperature is 0 to 100° C., preferably 25 to 35° C.; and / or the reaction time is 2 to 20 h, preferably 8 to 15 h.

[0028] The method of the present invention confines the benzyl functionalized ionic liquid in situ in the pores of MIL-101(Cr), thereby improving the performance of the benzyl functionalized ionic liquid. The catalyst prepared by the method of the present invention has the characteristics of improving the conversion rate of phenolic esters and the selectivity of hydroxyaromatic ketones.

[0029] The third aspect of the present invention provides a method for preparing hydroxy aromatic ketone from alkyl phenol ester or halogenated phenol ester, which comprises catalyzing the intramolecular rearrangement of alkyl phenol ester or halogenated phenol ester in solvent C or non-solvent state using the catalyst as described in the first aspect of the present invention or the catalyst prepared by the method described in the second aspect to synthesize hydroxy aromatic ketone.

[0030] In some embodiments of the present invention, the alkylphenol or halogenated phenol has a structural formula as shown in chemical formula a or chemical formula b;

[0031] Chemical formula a;

[0032] Chemical formula b;

[0033] Wherein, R2 and R3 are each independently selected from H or C1-C6 alkyl; R1 and R4 are each independently selected from C1-C6 alkyl or C6-C9 aryl; and X is selected from any one of F, Cl, Br and I.

[0034] In other embodiments of the present invention, the weight ratio of the alkylphenol ester or halogenated phenol ester to the catalyst is 1:(0.001-20); preferably 1:(0.01-5).

[0035] In some embodiments of the present invention, the solvent C is selected from any one of chlorobenzene, nitrobenzene, toluene, nitromethane, acetonitrile and dichloromethane.

[0036] In other embodiments of the present invention, the catalytic conditions include: temperature of 20-200°C, preferably 20-100°C; and / or pressure of normal pressure to 6MPa, preferably normal pressure to 2MPa; time of 0.1-10h, preferably 0.5-5h.

[0037] The beneficial effects of the present invention are as follows: the benzyl-functionalized ionic liquid in the catalyst of the present invention is in situ confined in the pores of the organometallic framework material (e.g., MIL-101(Cr)), thereby improving the performance of the benzyl-functionalized ionic liquid. The catalyst prepared by the method of the present invention is applied to the preparation of hydroxyaromatic ketones, which has the characteristics of improving the conversion rate of phenolic esters and the selectivity of hydroxyaromatic ketones. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The present invention will be further described below in conjunction with the accompanying drawings.

[0039] Figure 1 This is the XRD spectrum of the metal organic framework material MIL-101 (Cr) used in Example 1 of the present invention.

[0040] Figure 2 This is the XRD spectrum of the catalyst MIL-101(Cr)-Fe-1 prepared in Example 1 of the present invention.

[0041] Figure 3 This is the IR spectrum of the metal organic framework material MIL-101 (Cr) used in Example 1 of the present invention. The main peak position is: 3441 cm -1 、1653cm -1 、1617cm -1 、1505cm -1 、1384cm -1 、1106cm -1 、749cm -1 .

[0042] Figure 4 This is the IR spectrum of the organometallic catalyst MIL-101(Cr)-Fe-1 prepared in Example 1 of the present invention. The main peak position is: 3407cm -1 、3053cm -1 、1702cm -1 、1651cm -1 、1622cm -1 、1486cm -1 、1398cm -1 、1300cm -1 、1157cm -1 、1105cm -1 、1016cm -1 、749cm -1 、680cm -1 ; Among them, at 3053cm -1 The peak of benzyl group is 1702cm -1 The peak of benzene ring, 1398cm -1 、1157cm-1 、680cm -1 The peak of the pyridine ring is 1300 cm -1 、1016cm -1 It is the peak of benzylbenzene ring. DETAILED DESCRIPTION

[0043] In order to make the present invention easier to understand, the present invention will be further described in detail below in conjunction with examples, which are merely illustrative and are not intended to limit the scope of application of the present invention. The raw materials or components used in the present invention can be obtained by commercial routes or conventional methods unless otherwise specified.

[0044] [Preparation Example 1]

[0045] MIL-101(Cr)(XRD spectrum as shown Figure 1 As shown, the IR spectrum is Figure 3 The samples were dried in an oven at 150°C overnight.

[0046] In a dried 100 mL three-necked flask, add 25 mL of anhydrous acetonitrile, 2 g of dried MIL-101(Cr), and 0.25 mL of pyridine, and add 0.32 mL of benzyl chloride dropwise under stirring, and react at room temperature for 12 hours. Filter the system, wash the filter cake thoroughly with anhydrous acetonitrile, and vacuum dry to obtain a solid product.

[0047] The solid product was added to a 100 mL three-necked flask after drying, and 25 mL of anhydrous acetonitrile was added. 1 g of anhydrous ferric chloride was added under stirring, and the reaction was carried out at room temperature for 12 hours. The acetonitrile layer was separated, and then fully washed with anhydrous acetonitrile and dried in vacuum to obtain the catalyst MIL-101(Cr)-Fe-1 (XRD spectrum as shown in FIG. Figure 2 As shown, the IR spectrum is Figure 4 shown).

[0048] [Preparation Example 2]

[0049] The MIL-101(Cr) was dried in an oven at 150°C overnight.

[0050] In a dried 100 mL three-necked flask, add 25 mL of anhydrous acetonitrile, 2 g of dried MIL-101(Cr), and 0.25 mL of pyridine, and add 0.32 mL of benzyl chloride dropwise under stirring, and react at room temperature for 12 hours. Filter the system, wash the filter cake thoroughly with anhydrous acetonitrile, and vacuum dry to obtain a solid product.

[0051] The solid product was added to a dried 100 mL three-necked flask, and 25 mL of anhydrous acetonitrile was added. 0.82 g of aluminum chloride was added under stirring, and the reaction was carried out at room temperature for 12 hours. The acetonitrile layer was separated, and then fully washed with anhydrous acetonitrile and vacuum dried to obtain the catalyst MIL-101(Cr)-Al-1.

[0052] [Preparation Example 3]

[0053] The MIL-101(Cr) was dried in an oven at 150°C overnight.

[0054] In a dried 100 mL three-necked flask, add 25 mL of anhydrous acetonitrile, 2 g of dried MIL-101(Cr), and 0.25 mL of pyridine, and add 0.32 mL of benzyl chloride dropwise under stirring, and react at room temperature for 12 hours. Filter the system, wash the filter cake thoroughly with anhydrous acetonitrile, and vacuum dry to obtain a solid product.

[0055] The solid product was added to a dried 100 mL three-necked flask, and 25 mL of anhydrous acetonitrile was added. 0.84 g of zinc chloride was added under stirring, and the reaction was carried out at room temperature for 12 hours. The acetonitrile layer was separated, and then fully washed with anhydrous acetonitrile and vacuum dried to obtain the catalyst MIL-101(Cr)-Zn-1.

[0056] [Preparation Example 4]

[0057] The MIL-101(Cr) was dried in an oven at 150°C overnight.

[0058] In a dried 100 mL three-necked flask, add 25 mL of anhydrous acetonitrile, 2 g of dried MIL-101(Cr), and 0.25 mL of pyridine, and add 0.41 mL of trifluoromethylbenzyl chloride dropwise under stirring. React at room temperature for 12 hours. Filter the system, wash the filter cake thoroughly with anhydrous acetonitrile, and vacuum dry to obtain a solid product.

[0059] The solid product was added to a dried 100 mL three-necked flask, and 25 mL of anhydrous acetonitrile was added. 1 g of anhydrous ferric chloride was added under stirring, and the reaction was carried out at room temperature for 12 hours. The acetonitrile layer was separated, and then fully washed with anhydrous acetonitrile and vacuum dried to obtain the catalyst MIL-101(Cr)-Fe-2.

[0060] [Preparation Example 5]

[0061] The MIL-101(Cr) was dried in an oven at 150°C overnight.

[0062] In a dried 100 mL three-necked flask, add 25 mL of anhydrous acetonitrile, 2 g of dried MIL-101(Cr), and 0.25 mL of pyridine, and add 0.47 mL of p-isopropylbenzyl chloride dropwise under stirring. React at room temperature for 12 hours. Filter the system, wash the filter cake thoroughly with anhydrous acetonitrile, and vacuum dry to obtain a solid product.

[0063] The solid product was added to a dried 100 mL three-necked flask, and 25 mL of anhydrous acetonitrile was added. 1 g of anhydrous ferric chloride was added under stirring, and the reaction was carried out at room temperature for 12 hours. The acetonitrile layer was separated, and then fully washed with anhydrous acetonitrile and vacuum dried to obtain the catalyst MIL-101(Cr)-Fe-3.

[0064] [Preparation Example 6]

[0065] After drying, add 100 mL of anhydrous acetonitrile and 2.5 mL of pyridine to a 200 mL three-necked flask, add 3.2 mL of benzyl chloride dropwise while stirring, and react at room temperature for 12 hours. Add 10 g of anhydrous ferric chloride while stirring, and react at room temperature for 12 hours. Separate the acetonitrile layer, wash it thoroughly with anhydrous acetonitrile, and dry it in vacuum to obtain the catalyst PyBn-Fe.

[0066] [Comparative Example 1]

[0067] 2.5 mL of phenyl acetate and 0.4 g of dried PyBn-Fe prepared in Preparation Example 6 were added to a 50 mL flask, and the system was heated to 80°C for 4 hours and cooled to room temperature. 50 mL of water was added and stirred thoroughly, and then extracted three times with ethyl acetate. The organic phases were combined, dried over anhydrous Na2SO4, and then filtered. The solvent was evaporated under reduced pressure, and the residue was analyzed by GC. The conversion rate of phenyl acetate was 67.8%, and the selectivity of hydroxyacetophenone was 59.4%.

[0068] [Example 1]

[0069] 2.5 g of phenyl acetate and 1 g of dried MIL-101(Cr)-Fe-1 prepared in Preparation Example 1 were added to a 50 mL flask, and the system was heated to 80°C for 4 hours and cooled to room temperature. 50 mL of water was added and stirred thoroughly, and then extracted three times with ethyl acetate. The organic phases were combined, dried over anhydrous Na2SO4, and filtered. The solvent was evaporated under reduced pressure, and the residue was analyzed by GC. The conversion rate of phenyl acetate was 99.2%, and the selectivity of hydroxyacetophenone was 91.6%.

[0070] [Example 2]

[0071] 2.5 g of phenyl acetate and 1 g of dried MIL-101(Cr)-Al-1 prepared in Preparation Example 2 were added to a 50 mL flask, and the system was heated to 80°C for 4 hours and cooled to room temperature. 50 mL of water was added and stirred thoroughly, and then extracted three times with ethyl acetate. The organic phases were combined, dried over anhydrous Na2SO4, and then filtered. The solvent was evaporated under reduced pressure, and the residue was analyzed by GC. The conversion rate of phenyl acetate was 99.9%, and the selectivity of hydroxyacetophenone was 90.2%.

[0072] [Example 3]

[0073] 2.5 g of phenyl acetate and 1 g of the dried MIL-101(Cr)-Zn-1 system prepared in Preparation Example 3 were added to a 50 mL flask and heated to 80°C for 4 hours, then cooled to room temperature. 50 mL of water was added and stirred thoroughly, and then extracted three times with ethyl acetate. The organic phases were combined, dried over anhydrous Na2SO4, filtered, and the solvent was removed by distillation under reduced pressure. The residue was analyzed by GC. The conversion rate of phenyl acetate was 97.3%, and the selectivity of hydroxyacetophenone was 90.4%.

[0074] [Example 4]

[0075] 2.5 g of phenyl acetate and 1 g of dried MIL-101(Cr)-Fe-2 prepared in Preparation Example 4 were added to a 50 mL flask, and the system was heated to 80°C for 4 hours and cooled to room temperature. 50 mL of water was added and stirred thoroughly, and then extracted three times with ethyl acetate. The organic phases were combined, dried over anhydrous Na2SO4, and filtered. The solvent was evaporated under reduced pressure, and the residue was analyzed by GC. The conversion rate of phenyl acetate was 99.3%, and the selectivity of hydroxyacetophenone was 94.3%.

[0076] [Example 5]

[0077] 2.5 g of phenyl acetate and 1 g of dried MIL-101(Cr)-Fe-1 prepared in Preparation Example 5 were added to a 50 mL flask, and the system was heated to 80°C for 4 hours and cooled to room temperature. 50 mL of water was added and stirred thoroughly, and then extracted three times with ethyl acetate. The organic phases were combined, dried over anhydrous Na2SO4, and filtered. The solvent was evaporated under reduced pressure, and the residue was analyzed by GC. The conversion rate of phenyl acetate was 98.5%, and the selectivity of hydroxyacetophenone was 90.3%.

[0078] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.

Claims

1. A catalyst for preparing hydroxyaromatic ketone, comprising an organic metal framework material and a benzyl-functionalized ionic liquid; and the catalyst has the following X-ray diffraction pattern; in, (a)=±0.3°。 2. A catalyst for preparing hydroxyaromatic ketone, characterized in that: It comprises an organic metal framework material and a benzyl functionalized ionic liquid, wherein the organic metal framework material is selected from one or more of IRMOF, ZIFs, PCPs and MIL; the structure of the benzyl functionalized ionic liquid contains cations formed by nitrogen heterocyclic organic compounds and benzyl halide compounds and metal halides.

3. The catalyst according to claim 2, characterized in that The organic metal framework material is selected from MIL.

4. The catalyst according to claim 3, characterized in that The MIL is selected from one or more of MIL-53, MIL-100 and MIL-101.

5. The catalyst according to claim 4, characterized in that The MIL is selected from MIL-101.

6. The catalyst according to claim 5, characterized in that The MIL is selected from MIL-101(Cr).

7. A method for preparing a catalyst as claimed in any one of claims 1 to 6, comprising the following steps: S1, mixing solvent A, an organic metal framework material, a nitrogen heterocyclic organic compound and a benzyl halide compound, reacting the mixture, and then cooling, filtering, washing and drying the mixture to obtain a solid product; S2, mixing solvent B, the solid product and Lewis acid, and reacting the mixture, followed by cooling, filtering, washing and drying to obtain the catalyst.

8. The method according to claim 7, characterized in that The molar ratio of the nitrogen heterocyclic organic compound, the benzyl halide compound and the Lewis acid is (0.5-1.5):(0.5-1.5):(1.5-2.5).

9. The method according to claim 8, characterized in that The molar ratio of the nitrogen heterocyclic organic compound, the benzyl halide compound and the Lewis acid is (0.8-1.2):(0.8-1.2):(1.8-2.2).

10. The method according to any one of claims 7 to 9, characterized in that: The nitrogen heterocyclic organic compound is selected from one or more of imidazole, alkylimidazole, pyridine, alkylpyridine, pyrimidine, alkylpyrimidine, pyrrole and alkylpyrrole; and / or The benzyl halide compound is selected from one or more of benzyl chloride, 2,4,6-trimethylbenzyl chloride, p-trifluoromethylbenzyl chloride, benzyl bromide and 4-isopropylbenzyl bromide; and / or The Lewis acid is selected from one or more of aluminum trichloride, aluminum tribromide, ferric chloride, zinc chloride, boron trifluoride, gallium chloride, indium chloride, and cuprous chloride; and / or The solvent A and the solvent B are each independently selected from any one of chlorobenzene, nitrobenzene, toluene, nitromethane, acetonitrile and dichloromethane.

11. The method according to claim 10, characterized in that The alkyl group is selected from at least one of C1 to C5 alkyl groups; and / or The Lewis acid is selected from one or more of aluminum chloride and ferric chloride.

12. The method according to claim 11, characterized in that The nitrogen heterocyclic organic compound is selected from one or more of pyridine, 4-methylpyridine, 3-methylpyridine and 3,5-dimethylpyridine.

13. The method according to any one of claims 7 to 9, characterized in that: In step S1, the reaction temperature is 0 to 100° C.; and / or the reaction time is 2 to 72 hours; and / or In step S2, the reaction temperature is 0 to 100° C.; and / or the reaction time is 2 to 20 hours.

14. The method according to claim 13, characterized in that In step S1, the reaction temperature is 30-40°C; and / or the reaction time is 12-15h; and / or In step S2, the reaction temperature is 25-35° C.; and / or the reaction time is 8-15 h.

15. A method for preparing hydroxy aromatic ketone from alkylphenol ester or halogenated phenol ester, comprising catalyzing intramolecular rearrangement of alkylphenol ester or halogenated phenol ester using a catalyst as claimed in any one of claims 1 to 6 or a catalyst prepared by the method as claimed in any one of claims 7 to 14 in a solvent C or a non-solvent state, thereby synthesizing hydroxy aromatic ketone.

16. The method according to claim 15, characterized in that The alkylphenol ester or halogenated phenol ester has a structural formula as shown in chemical formula a or chemical formula b; Wherein, R2 and R3 are each independently selected from H or C1-C6 alkyl; R1 and R4 are each independently selected from C1-C6 alkyl or C6-C9 aryl; X is selected from any one of F, Cl, Br and I; And / or, the weight ratio of the alkylphenol ester or halogenated phenol ester to the catalyst is 1:(0.001-20).

17. The method according to claim 16, characterized in that The weight ratio of the alkylphenol ester or halogenated phenol ester to the catalyst is 1:(0.01-5).

18. The method according to any one of claims 15 to 17, characterized in that: The solvent C is selected from any one of chlorobenzene, nitrobenzene, toluene, nitromethane, acetonitrile and dichloromethane; and / or The catalytic conditions include: temperature of 20-200° C.; and / or pressure of normal pressure to 6 MPa; and time of 0.1-10 h.

19. The method according to claim 18, characterized in that The catalytic conditions include: a temperature of 20 to 100° C.; and / or a pressure of normal pressure to 2 MPa; and / or a time of 0.5 to 5 hours.

Citation Information

Patent Citations

  • Metal organic framework material / functional ionic liquid composite material as well as preparation and application thereof

    CN106693899A

  • Mercury-free catalyst used for addition reactionof acetylene with hydrogen chloride and preparation method of mercury-free catalyst

    CN106914276A