A modified silver-coated metal powder and preparation method thereof
By heating and stirring the silver-clad metal powder in the active solution, the problem of incomplete coating of cheap silver-clad metal powder is solved, and higher cladding and stability are achieved, and electrical performance and service life are improved.
Patent Information
- Application Number
- CN202310027683.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-01-09
AI Technical Summary
The incomplete coating of existing silver-clad cheap metal powder causes the resistance and aging performance to be affected, and the leakage of cheap metals is prone to occur during use, affecting the electrical performance.
By adding silver-clad metal powder to the solvent and heating and stirring in the active solution, the metal oxide is removed by using the active substance to promote silver coating, achieving complete coverage of silver to the cheap metal surface and reducing coating defects.
It significantly improves the cladding degree of cheap metal powder in silver-clad bags, reduces the exposure of cheap metal oxides, improves conductive properties and thermodynamic stability, and extends service life.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silver-coated metal powders, and in particular to modified silver-coated metal powders and a preparation method thereof. Background Art
[0002] At present, with the emergence of silver-coated cheap metal powder, the status of silver as the most important conductive metal in the paste is gradually reduced. The large-scale use of mainstream silver-coated cheap metal powders, such as silver-coated copper powder and silver-coated nickel powder, has further reduced the cost of metal conductive paste. In the case that the conductivity of cheap metals is not much different from that of silver, they can be widely used in most fields that do not require high electrical properties to replace the silver powder used in traditional silver paste and silver glue.
[0003] The current mainstream silver-coated cheap metal powder is mainly prepared by three methods: ball milling, melting and chemical methods. Among them, the chemical method is the most widely used method in terms of coating integrity, process stability and comprehensive product performance. Silver salt and cheap metal or reducing agent undergo redox reaction so that silver is coated on the surface of cheap metal. However, even the chemical method cannot make silver completely coat cheap metal. Incomplete coating will further affect resistance and aging performance, which limits the use of silver-coated cheap metal.
[0004] At present, the downstream slurry manufacturers of silver-coated cheap metal powders directly mix the silver-coated cheap metal powders for use without any surface treatment. This results in some cheap metal powders with incomplete coatings. They may not cause major problems in the early use tests, but will leak cheap metal during the later use and aging process, thus affecting the most basic electrical properties.
[0005] Based on the defects of the current silver-coated cheap metal powder, it is necessary to modify it. Summary of the invention
[0006] In view of this, the present invention proposes a modified silver-coated metal powder and a preparation method thereof to solve the technical problem that diniconazole is poorly soluble in water in the prior art.
[0007] In a first aspect, the present invention provides a modified silver-coated metal powder, comprising the following components: silver-coated metal powder, a solvent and an active substance;
[0008] The solvent includes at least one of water, methanol, isopropanol, butanol, ethylene glycol, ethyl acetate, butyl acetate, toluene, xylene, formic acid, acetic acid, acetone, butanone, methyl butanone, cyclohexanone, DBE, MDBE, dimethylformamide, ethylene glycol monomethyl ether, diethylene glycol dimethyl ether, diethylene glycol butyl ether acetate, diethylene glycol butyl ether, octanol, octyl acetate, terpineol, isophorone, ethylene glycol monoethyl ether, and acetonitrile;
[0009] The active substance includes at least one of an acid solution, a reducing agent, a protective ligand, and a silver salt.
[0010] Preferably, in the modified silver-coated metal powder, the acid solution includes at least one of sulfuric acid, hydrochloric acid, nitric acid, lactic acid, acetic acid, benzoic acid, succinic acid, carbonic acid, stearic acid, oleic acid, and palmitic acid.
[0011] Preferably, in the modified silver-coated metal powder, the reducing agent includes at least one of formaldehyde, acetaldehyde, sodium hydroxide, potassium hydroxide, oxalic acid, sodium borohydride, potassium borohydride, copper, iron, aluminum, nickel, polysaccharides, starch, glucose, hydrogen peroxide, ascorbic acid, ethylene glycol, hydrazine hydrate, ammonia water, ferrous sulfate, and 1-methyl-3-butylimidazole tetrafluoroborate.
[0012] Preferably, in the modified silver-coated metal powder, the protective ligand includes at least one of thiol compounds, amino compounds, carboxyl compounds, hydrogen sulfide, sulfuric acid, dimethyl sulfoxide, ammonia water, dimethylformamide, acetate, phenol, water, and basic copper carbonate.
[0013] Preferably, the modified silver-coated metal powder comprises at least one of silver-coated copper powder and silver-coated nickel powder.
[0014] Preferably, the modified silver-coated metal powder has a particle size of 0.25 to 20 μm.
[0015] Preferably, in the modified silver-coated metal powder, the mass ratio of the silver-coated metal powder, the solvent and the active substance is (10-95):(5-100):(1-30).
[0016] In a second aspect, the present invention further provides a method for preparing the modified silver-coated metal powder, comprising the following steps:
[0017] The silver-coated metal powder is added into a solvent, and then an active substance is added, and the mixture is stirred for reaction to obtain the modified silver-coated metal powder.
[0018] Preferably, in the method for preparing the modified silver-coated metal powder, the silver-coated metal powder is added to a solvent, and then an active substance is added, and in the step of stirring the reaction, the stirring rate is 50 to 5000 rpm.
[0019] Preferably, in the preparation method of the modified silver-coated metal powder, the silver-coated metal powder is added to a solvent, and then an active substance is added, and in the step of stirring the reaction, the reaction temperature is 25 to 200° C. and the reaction time is 15 min to 48 h.
[0020] The modified silver-coated metal powder and the preparation method thereof of the present invention have the following beneficial effects compared with the prior art:
[0021] The modified silver-coated metal powder of the present invention comprises silver-coated metal powder, solvent and active substance. By adding the silver-coated metal powder into the solvent and then adding the active substance, in a solution with a certain activity, the oxide on the metal surface is easily removed by the reducing substance, thereby exposing the surface of the cheap metal with higher activity; and silver is more easily coated on the newly generated cheap metal surface under the induction of the active substance at a high temperature, thereby realizing the coating of the cheap metal by silver; in the process of repeatedly removing the cheap metal oxide and coating the silver, the complete coating of the cheap metal surface by silver is realized, and the final thermodynamically stable state is achieved. The present invention soaks the silver-coated metal powder in a solution with a certain activity and heats it, thereby greatly reducing the vacancies on the surface of the silver-coated cheap metal. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] The present invention provides a modified silver-coated metal powder, comprising the following components: silver-coated metal powder, solvent and active substance;
[0024] The solvent includes at least one of water, methanol, isopropanol, butanol, ethylene glycol, ethyl acetate, butyl acetate, toluene, xylene, formic acid, acetic acid, acetone, butanone, methyl butanone, cyclohexanone, DBE, MDBE, dimethylformamide, ethylene glycol monomethyl ether, diethylene glycol dimethyl ether, diethylene glycol butyl ether acetate, diethylene glycol butyl ether, octanol, octyl acetate, terpineol, isophorone, ethylene glycol monoethyl ether, and acetonitrile;
[0025] The active substance includes at least one of an acid solution, a reducing agent, a protective ligand, and a silver salt.
[0026] It should be noted that the silver-coated metal powder of the present application is the target powder that needs to improve the coating, which is the silver-coated cheap metal powder purchased directly from the market, including silver-coated copper powder, silver-coated nickel powder, etc.; the solvent plays the role of dispersing the silver-coated cheap metal powder, and the type of solvent is optimal for dispersing the silver-coated cheap metal powder; the role of the active substance is to activate the surface silver and cheap metal of the silver-coated cheap metal, so that it can move slowly under heating conditions, and make the silver coated on the surface of the cheap metal. Since the melting point of silver reaches 960°C, without adding active substances, the thicker silver layer is very difficult to move and complete the coating at a lower temperature.
[0027] Specifically, DBE solvent (named DBE by DuPont) is a mixture of three divalent acid esters, commonly known as nylon acid methyl ester, which is a combination of three good environmental solvents: dimethyl succinate (butanedioic acid) CH3OOC(CH2)2COOCH3, dimethyl glutarate CH3OOC(CH2)3COOCH3 and dimethyl adipate CH3OOC(CH2)4COOCH3.
[0028] In some embodiments, the acid solution includes at least one of sulfuric acid, hydrochloric acid, nitric acid, lactic acid, acetic acid, benzoic acid, succinic acid, carbonic acid, stearic acid, oleic acid, and palmitic acid.
[0029] In some embodiments, the reducing agent includes at least one of formaldehyde, acetaldehyde, sodium hydroxide, potassium hydroxide, oxalic acid, sodium borohydride, potassium borohydride, copper, iron, aluminum, nickel, polysaccharides, starch, glucose, hydrogen peroxide, ascorbic acid, ethylene glycol, hydrazine hydrate, ammonia water, ferrous sulfate, and 1-methyl-3-butylimidazole tetrafluoroborate.
[0030] In some embodiments, the protective ligand includes at least one of a thiol compound, an amino compound, a carboxyl compound, hydrogen sulfide, sulfuric acid, dimethyl sulfoxide, ammonia, dimethylformamide, acetate, phenol, water, and basic copper carbonate.
[0031] In some embodiments, the silver salt includes at least one of silver nitrate, silver oxide, silver acetate, silver sulfate, silver chloride, silver bromide, silver iodide, silver ammonium, silver carbonate, silver lactate, silver stearate, and silver phosphate.
[0032] In some embodiments, the silver-coated metal powder includes at least one of silver-coated copper powder and silver-coated nickel powder.
[0033] In some embodiments, the particle size of the silver-coated metal powder is 0.25-20 μm.
[0034] In some embodiments, the mass ratio of the silver-coated metal powder, the solvent, and the active substance is (10-95):(5-100):(1-30).
[0035] Based on the same inventive concept, the present application also provides a method for preparing the modified silver-coated metal powder, comprising the following steps:
[0036] The silver-coated metal powder is added into a solvent, and then an active substance is added, and the mixture is stirred for reaction to obtain the modified silver-coated metal powder.
[0037] The preparation method of the modified silver-coated metal powder of the present application aims to improve the coating degree of the silver-coated cheap metal powder, and to perform certain pretreatment on the surface of the directly purchased silver-coated cheap metal powder, so as to achieve a higher coating degree of the silver-coated cheap metal; the pretreatment method is to immerse the silver-coated cheap metal powder in a solution with a certain activity and heat it, so that the vacancies on the surface of the silver-coated cheap metal are greatly reduced; specifically, the reaction principle of the present application is: due to the incomplete coating of silver, the cheap metal (such as copper, nickel, etc.) is exposed to the air, and it is easy to form cheap metal oxides, thereby affecting the conductivity of the silver-coated metal powder. At the same time, due to the mismatch between the metal oxide and the silver lattice, it is difficult for silver to cover its surface during further coating, thereby causing defects; and in a solution with a certain activity, the oxide on the metal surface is easily removed by the reducing substance, thereby exposing the surface of the cheap metal with higher activity. Silver is more likely to be coated on the newly generated cheap metal surface under the induction of the active substance at a high temperature, thereby achieving the coating of the cheap metal by silver. In the process of repeatedly removing cheap metal oxides and coating silver, the silver is completely coated on the surface of the cheap metal, reaching the final thermodynamically stable state. The incomplete coating state is due to the excessive activity of the reactants, which generates substances with kinetic reactions, resulting in incomplete coating.
[0038] In some embodiments, silver-coated metal powder is added to a solvent, and then an active substance is added. In the step of stirring the reaction, the stirring rate is 50 to 5000 rpm. The main purpose of stirring is to make the overall reaction more uniform, so the stirring speed is related to the viscosity of the liquid, generally 50 to 5000 rpm. If the stirring speed is too slow, the reaction is not uniform enough. If the stirring speed is too fast, it is easy to cause shearing of the powder, thereby affecting the morphology and easily generating kinetic products.
[0039] In some embodiments, silver-coated metal powder is added to a solvent, and then an active substance is added. In the step of stirring the reaction, the reaction temperature is 25 to 200°C and the reaction time is 15 min to 48 h. The heating temperature is a very important parameter, which directly determines the speed of the reaction and the direction of the reaction. The temperature is generally selected from 25 to 200°C. If the temperature is too low, the reaction speed is too slow, and the surface of the silver-coated cheap metal may be difficult to change. If the temperature is too high, the reaction activity is too high, resulting in more reaction products in the kinetic direction, affecting the coating effect of the silver-coated cheap metal. The purpose of heating is to speed up the reaction speed, so the time and temperature are also related, generally 15 min to 48 h. If the time is too short, the reaction does not occur. If the time is too long, it is not friendly to the efficiency of the reaction. There are certain problems in the setting of conditions.
[0040] Specifically, the mass ratio of silver-coated metal powder, solvent and active substance is (10-95):(5-100):(1-30); the amount of silver-coated metal powder added is 10-95 parts by weight. If too little silver-coated metal powder is added, the coating efficiency is too low and it is difficult to mass produce. If too much silver-coated metal powder is added, the viscosity is too high and it is difficult to improve the surface. The particle size of the silver-coated metal powder is 0.25-20 μm. If the particle size of the silver-coated metal powder is too small, the powder activity of the silver-coated metal powder is too high, and the coating is difficult. Powders with too large diameters generally have better coating properties, but are rarely used downstream and are generally not considered. The amount of solvent added is 5-100 parts by weight. If too little solvent is added, the viscosity is too high and it is difficult to stir evenly. If too much solvent is added, the efficiency is too low and it is difficult to mass produce. The amount of active substance added is 1-30 parts. If too little solvent is added, the reaction will be difficult to carry out, affecting the coating effect. If too much solvent is added, the reaction speed will be too fast, and it is easy to produce substances with kinetic reactions, thereby making the coating worse.
[0041] Specifically, the silver-coated metal powder is added to a solvent, and then the active substance is added, stirred for reaction, filtered, and dried to obtain the modified silver-coated metal powder.
[0042] The following further illustrates the preparation method and application of the modified silver-coated metal powder of the present application with specific examples. This section further illustrates the content of the present invention in conjunction with specific examples, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means adopted in the examples are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0043] Example 1
[0044] The present invention provides a method for preparing a modified silver-coated metal powder, comprising the following steps:
[0045] 80 parts by weight of commercially available silver-coated copper powder (the mass fraction of silver in the silver-coated copper powder is 20% and the average particle size of the silver-coated copper powder is 5 μm) are added to 10 parts by weight of ethylene glycol solvent, and then 2 parts by weight of an aqueous nitric acid solution with an active substance pH of 2 is added. The reaction is stirred at a stirring rate of 1000 rpm and a temperature of 120°C for 3 hours, and the mixture is filtered and dried to obtain a modified silver-coated copper powder.
[0046] Example 2
[0047] The present invention provides a method for preparing a modified silver-coated metal powder, comprising the following steps:
[0048] 80 parts by weight of commercially available silver-coated copper powder (the silver mass fraction in the silver-coated copper powder is 20% and the average particle size of the silver-coated copper powder is 5 μm) is added to a mixed solvent consisting of 7 parts by weight of water and 7 parts by weight of isopropanol, and then 5 parts by weight of an aqueous solution of oxalic acid with a pH value of 2 as an active substance is added. The reaction is stirred at a stirring rate of 1000 rpm and a temperature of 120°C for 3 hours, and the mixture is filtered and dried to obtain a modified silver-coated copper powder.
[0049] Example 3
[0050] The present invention provides a method for preparing a modified silver-coated metal powder, comprising the following steps:
[0051] 60 parts by weight of commercially available silver-coated copper powder (the silver mass fraction in the silver-coated copper powder is 20% and the average particle size of the silver-coated copper powder is 5 μm) are added to a mixed solvent consisting of 15 parts by weight of DBE and 5 parts by weight of isophorone, and then an active substance consisting of 1.5 parts by weight of p-mercaptobenzoic acid and 1.5 parts by weight of p-aminobenzoic acid is added. The reaction is stirred at a stirring rate of 500 rpm and a temperature of 150°C for 1 hour, and the mixture is filtered and dried to obtain a modified silver-coated copper powder.
[0052] Example 4
[0053] The present invention provides a method for preparing a modified silver-coated metal powder, comprising the following steps:
[0054] 80 parts by weight of commercially available silver-coated nickel powder (the mass fraction of silver in the silver-coated nickel powder is 20% and the average particle size of the silver-coated nickel powder is 5 μm) are added to 10 parts by weight of ethyl acetate solvent, and then 2 parts by weight of active substance silver acetate are added. The reaction is stirred at a stirring rate of 1000 rpm and a temperature of 80°C for 3 hours, and the mixture is filtered and dried to obtain modified silver-coated nickel powder.
[0055] Comparative Example 1
[0056] The present invention provides a method for preparing a modified silver-coated metal powder, comprising the following steps:
[0057] 80 parts by weight of commercially available silver-coated copper powder (the mass fraction of silver in the silver-coated copper powder is 20% and the average particle size of the silver-coated copper powder is 5 μm) are added to 10 parts by weight of ethylene glycol solvent, stirred and reacted for 3 hours at a stirring rate of 1000 rpm and a temperature of 25°C (i.e., room temperature), filtered and dried to obtain modified silver-coated copper powder.
[0058] Performance Testing
[0059] In the above-mentioned Examples 1 to 4, aqueous nitric acid solution is used as the active substance in Example 1, aqueous oxalic acid solution as the reducing agent is used as the active substance in Example 2, ligands p-mercaptobenzoic acid and p-aminobenzoic acid are used as the active substances in Example 3, and silver salt silver acetate is used as the active substance in Example 4; the modified silver-coated copper powder prepared in Examples 1 to 3, the modified silver-coated nickel powder prepared in Example 4, the modified silver-coated copper powder prepared in Comparative Example 1, and the commercially available silver-coated copper powder used in Example 1 (as Comparative Example 2) are tested for silver coating; the specific testing method is: 1 part by weight of the modified silver-coated metal powder prepared in different Examples or 1 part by weight of the commercially available silver-coated copper powder are respectively added to 10 parts by weight of hydrochloric acid solution with a pH of 3, stirred for 1 hour, and the copper ion (or nickel ion) content in the liquid is tested by ICP to determine the effect of the silver coating, and the results are shown in Table 1 below.
[0060] Table 1 - ICP test metal content in different examples
[0061] Example ICP test metal content (mg / mL) Example 1 7 Example 2 4 Example 3 3 Example 4 3 Comparative Example 1 38 Comparative Example 2 40
[0062] As can be seen from Table 1, in Example 1, by adding solvents and active substances and heating and stirring, partial silver-coated copper was repaired. Compared with the unrepaired Comparative Example 2, the amount of leaked copper was reduced by 33 mg / mL. At the same time, by comparing Example 2 with Example 1, it can be found that more reducing active agents can better repair the surface of the silver-coated copper, so that the detected copper ion content is almost reduced by half. Comparing Example 1 and Example 3, higher temperatures, more solvents, and more active surfactants can better assist silver in coating optimization, and the coating integrity is one order of magnitude better than that of Comparative Example 2. In Comparative Example 4, silver-coated nickel powder and acetate were used as active substances, and good repair effects were also obtained. Compared with Comparative Example 2, Comparative Example 1 has a poor coating effect in the absence of heating and active substances, and only stirring cannot achieve coating optimization. The final copper ion content of the modification method in Example 3 is the lowest, which is the optimal embodiment.
[0063] The above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing modified silver-coated metal powder, characterized in that: The modified silver-coated metal powder comprises the following components: silver-coated metal powder, solvent and active substance; Wherein, the solvent is a mixed solvent consisting of water and isopropanol; or, the solvent is a mixed solvent consisting of DBE and isophorone; The active substance includes at least one of a reducing agent and a protective ligand; The reducing agent is oxalic acid; The protective ligands are p-mercaptobenzoic acid and p-aminobenzoic acid; The silver-coated metal powder includes at least one of silver-coated copper powder and silver-coated nickel powder; The particle size of the silver-coated metal powder is 0.25-20 μm; The mass ratio of the silver-coated metal powder, the solvent and the active substance is (10-95):(5-100):(1-30); The preparation method of the modified silver-coated metal powder comprises the following steps: Adding silver-coated metal powder into a solvent, then adding active substances, stirring and reacting, thereby obtaining modified silver-coated metal powder; The silver-coated metal powder is added to the solvent, and then the active substance is added, and in the step of stirring the reaction, the reaction temperature is 120-150° C. and the reaction time is 1-3 hours.
2. The method for preparing the modified silver-coated metal powder according to claim 1, characterized in that: The silver-coated metal powder is added to the solvent, and then the active material is added. In the step of stirring the reaction, the stirring rate is 50-5000 rpm.
Citation Information
Cited By
Silver-coated copper powder surface modification method for low-temperature slurry
CN120362481A