An oriented porous piezoelectric ceramic catalyst and its preparation method and application
By adopting a piezoelectric ceramic catalyst with a oriented porous structure and combining with the preparation method of barium strontium titanate ceramic powder, the problem of difficult recovery of catalysts and insufficient specific surface area in the prior art is solved, and efficient decomposition of aquatic hydrogen and recyclability are achieved. sex.
Patent Information
- Application Number
- CN202211481584.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-11-24
AI Technical Summary
In the prior art, piezoelectric ceramic catalysts have problems that are difficult to recover during the decomposition of water and hydrogen production, and their specific surface area is insufficient, which affects the hydrogen production efficiency.
Using a piezoelectric ceramic catalyst with an oriented porous structure, the width of the ceramic sheet layer and the width of the pores can be controlled to achieve high specific surface area and high pore connectivity. Combined with the preparation method of barium strontium titanate ceramic powder, the volume porosity is controlled at 30. Within the range of ~50%, increase the hydrogen production rate of the catalyst.
A piezoelectric ceramic catalyst with high specific surface area and high pore connectivity is achieved, which improves the rate and efficiency of decomposition of aquatic hydrogen, is recyclable, and shows high decomposition of aquatic hydrogen under ultrasonic conditions.
Smart Images

Figure CN115845829B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an oriented porous piezoelectric ceramic catalyst and a preparation method and application thereof, belonging to the technical field of catalyst preparation. Background Art
[0002] In recent years, the use of piezoelectric materials to drive thermodynamically forbidden chemical reactions has become a new low-carbon and environmentally friendly means. For example, it can collect low-grade mechanical energy to catalyze the conversion of substances such as water and carbon dioxide into substances that are beneficial to the human body, thereby realizing the conversion of mechanical energy into electrical energy. Therefore, piezoelectric materials have great potential in the field of water decomposition to produce hydrogen.
[0003] Patent CN202111367520 discloses a tin, cerium-strontium titanate solid solution piezoelectric hydrogen production catalyst and its preparation method and application. The piezoelectric ceramic provided is a solid solution powder material. With the continuous improvement of laws and regulations related to environmental protection, piezoelectric ceramic powders used as catalysts to decompose water and produce hydrogen are often difficult to recycle and cause secondary pollution. Therefore, the use of block materials as catalysts has become a future trend. In addition, the bulk material can also be modified in a variety of ways to improve its hydrogen production efficiency. Patent CN202110118320 discloses a pn-BaTiO3 / NiO heterojunction piezoelectric ceramic, its preparation method and its application in self-powered and efficient hydrogen production. The catalyst provided is a dense ceramic block material with recyclability, but the specific surface area still needs to be improved.
[0004] There is no report on the use of porous piezoelectric ceramics to decompose water to produce hydrogen in the prior art. Summary of the invention
[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide an oriented porous piezoelectric ceramic catalyst and a preparation method and application thereof. The oriented porous piezoelectric ceramic catalyst prepared by the present invention has recyclability, high specific surface area, high pore connectivity, and solid-liquid separation ability.
[0006] In order to achieve the above objectives, this plan adopts the following technical solutions:
[0007] The invention discloses an oriented porous piezoelectric ceramic catalyst, which is an oriented porous structure. The oriented porous structure is composed of ceramic sheets with a width of 10 to 80 μm and arranged in parallel. The width of the pores between the ceramic sheets is 20 to 70 μm.
[0008] The oriented porous piezoelectric ceramic catalyst provided by the present invention has an oriented porous structure composed of ceramic sheets with a width of 10 to 80 μm arranged in parallel. The pores run through the part close to the bottom of the sample to the top of the sample. The sheets are filled with air. The sheets have high connectivity, which can realize material and energy exchange with the external environment. The reactant water molecules enter the pores to participate in the catalytic reaction, which can greatly increase the rate of hydrogen production by decomposing water.
[0009] Of course, to obtain an excellent rate of hydrogen production by decomposing water, both the thickness of the ceramic layer and the width of the pores need to be effectively controlled. If the ceramic layer is too narrow, the porosity of the sample will be high, the mechanical strength will decrease, and the piezoelectric ceramic phase will also decrease; if the ceramic layer is too thick, the pores will become fewer, which is not conducive to the material exchange between reactants and products, and the hydrogen production efficiency will be reduced. If the pore width is too large, the porosity of the sample will be high, the mechanical strength will decrease, and the piezoelectric ceramic phase will be reduced; if the pores are too small, it will be not conducive to the material exchange between reactants and products, and the hydrogen production efficiency will be reduced.
[0010] In a preferred embodiment, the volume porosity of the oriented porous piezoelectric ceramic catalyst is 30 to 50%, preferably 30 to 40%, and more preferably 40%.
[0011] In the present invention, by controlling the volume porosity of the oriented porous piezoelectric ceramic catalyst within the above range, the hydrogen production rate of the final material is optimal. If the porosity is too large or too small, the hydrogen production efficiency will be reduced. This is because if the porosity is too large, the mechanical strength will decrease, the content of the piezoelectric ceramic phase will also decrease accordingly, and the content of the effective part in the catalyst will decrease, resulting in a decrease in the hydrogen production efficiency. If the porosity is too small, there is no way to provide sufficient space for the consumption of reactants and the release of products, which is not conducive to the exchange of substances in the catalytic process and will also cause a decrease in the hydrogen production efficiency.
[0012] In a preferred embodiment, the thickness of the oriented porous piezoelectric ceramic catalyst is 1 to 1.5 mm.
[0013] In the present invention, there are no excessive restrictions on the specific composition of the piezoelectric ceramic in the oriented porous piezoelectric ceramic catalyst. The oriented porous piezoelectric ceramic catalyst under the above-mentioned structure has a good hydrogen production effect.
[0014] In a preferred embodiment, the ceramic in the piezoelectric ceramic catalyst is selected from at least one of barium strontium titanate, barium titanate, and barium calcium zirconate titanate, preferably barium strontium titanate. The ceramic of this preferred embodiment is used to obtain an oriented porous piezoelectric ceramic catalyst with the best hydrogen production efficiency.
[0015] In a preferred embodiment, the hydrogen production rate of the oriented porous piezoelectric ceramic catalyst is ≥100 nmol / h, preferably 400 nmol / h.
[0016] The invention discloses a method for preparing an oriented porous piezoelectric ceramic catalyst. The method comprises the following steps: mixing barium strontium titanate ceramic powder, water, a dispersant and an adhesive to obtain a ceramic slurry, placing the ceramic slurry in a mold, cooling the mold to -90 to -20°C at a cooling rate of 5 to 20°C / min, freezing the mold for 15 to 30 minutes, and then drying the mold at -50 to 0°C and 1 to 100 Pa to obtain a blank with an oriented porous structure. The blank is sintered to obtain the oriented porous piezoelectric ceramic catalyst.
[0017] The oriented porous piezoelectric ceramic catalyst of the present invention is prepared by preparing a ceramic slurry, pouring the ceramic slurry into a mold, converting the slurry into a raw material body with an oriented porous structure under a temperature gradient, placing the raw material body in a muffle furnace, performing high-temperature synthesis under a controlled reaction environment, and then cutting to obtain the oriented porous piezoelectric ceramic catalyst. The inventors have found that in the present invention, it is necessary to effectively control the freezing process. If the freezing temperature is high, the supercooling is small, and the growth rate of the solidified crystal is greater than its nucleation rate, which is more conducive to the growth of the solidified crystal, so that the pore size of the porous ceramic is larger; otherwise, the pore size is smaller. Therefore, the cooling rate and the final freezing rate need to be controlled within the scope of the present invention to avoid the pore size of the porous ceramic being too large or too small.
[0018] In a preferred embodiment, the particle size of the barium strontium titanate ceramic powder is 1 to 3 μm.
[0019] By controlling the particle size of barium strontium titanate ceramic powder within the above range, the performance of the final porous piezoelectric ceramic catalyst will be optimal. If the particle size is too large, the contact between the particles is insufficient, the filling is uneven, and the grains are easily not tightly bonded after sintering. Particles that are too fine are prone to adsorbing a large amount of gas, hindering the contact between the particles and also hindering sintering.
[0020] In a preferred embodiment, the preparation process of the barium strontium titanate ceramic powder is as follows: strontium carbonate, barium carbonate and titanium dioxide are prepared to obtain a mixed powder, the mixed powder is subjected to a first wet ball milling to obtain a suspension, the suspension is dried, and then a solid phase reaction is performed to obtain powder A, powder A is subjected to a second wet ball milling to obtain powder B, and powder B is dried and sieved to obtain barium strontium titanate ceramic powder.
[0021] Further preferably, in the mixed powder, the molar ratio is Ba:Sr:Ti:O=Ba:Sr:Ti:O=x:(1-x):1:3.
[0022] More preferably, in the mixed powder, the molar ratio of strontium carbonate: barium carbonate: titanium dioxide is 3:1:12.
[0023] Further preferably, the medium for the first wet ball milling is anhydrous ethanol.
[0024] More preferably, the temperature of the solid phase reaction is 1200-1320° C., and the time of the solid phase reaction is 2-4 hours.
[0025] Further preferably, the medium for the second wet ball milling is anhydrous ethanol.
[0026] Further preferably, the rotation speed of the second wet ball milling is 250-350 r / min, and the time of the second wet ball milling is 36-72 h.
[0027] In a preferred embodiment, the dispersant is selected from at least one of ammonium citrate, tetramethylammonium hydroxide, ammonium polyacrylate, and polyacrylate.
[0028] In a preferred embodiment, the adhesive is selected from at least one of polyvinyl alcohol, polyvinyl pyrrolidone, polyvinyl butyral, and carboxymethyl cellulose.
[0029] In a preferred embodiment, in the ceramic slurry, the volume fraction of the barium strontium titanate ceramic powder is 30 vol.% to 50 vol.%.
[0030] The inventors have discovered that the volume fraction of barium strontium titanate ceramic powder has a significant influence on the structure of the ultimately formed oriented porous piezoelectric ceramic catalyst. Only by controlling the volume fraction within the scope of the present invention can the structure required by the present invention be obtained, and ultimately an ideal hydrogen production efficiency be obtained. If the solid content is too high, the slurry viscosity will be high, the resistance that ice crystal growth needs to overcome will be greater, the thickness of the ceramic layer will increase, while the width of the pores will decrease, and the porosity will decrease. In addition, an excessively high solid content will also prevent the slurry from obtaining good dispersion in the suspension. If the solid content is too low, the slurry viscosity will be low, the thickness of the ceramic layer will decrease, while the width of the pores will increase, and the porosity will increase.
[0031] In a preferred embodiment, the amount of the dispersant added is 0.5-2% of the mass of the barium strontium titanate ceramic powder.
[0032] In a preferred embodiment, the amount of the adhesive added is 0.5-2% of the mass of the barium strontium titanate ceramic powder.
[0033] In a preferred embodiment, the sintering process is to first heat the temperature to 550-650°C at a heating rate of 1-3°C / min and keep it at that temperature for 2-4 hours, and then heat the temperature to 1200-1320°C at a heating rate of 3-5°C / min and keep it at that temperature for 2-4 hours.
[0034] In the sintering process of the present invention, a slower heating rate is adopted in the first stage, and the organic additives are removed evenly and completely by keeping the temperature at 550-650°C, and then the temperature is raised to 1200-1320°C and sintered to obtain an oriented porous piezoelectric ceramic catalyst. Of course, the final sintering temperature also needs to be effectively controlled. If the sintering temperature is too high or too low, the performance of the ceramic catalyst will be reduced.
[0035] The invention discloses an application of an oriented porous piezoelectric ceramic catalyst, wherein the oriented porous piezoelectric ceramic catalyst is applied to catalytically decomposing water to produce hydrogen.
[0036] The preferred solution and application process are as follows: placing the oriented porous piezoelectric ceramic catalyst in pure water and catalytically decomposing it under ultrasonic conditions to produce hydrogen.
[0037] Beneficial Effects
[0038] The present invention provides an oriented porous piezoelectric ceramic catalyst. The oriented porous structure is composed of ceramic sheets with a width of 10 to 80 μm and arranged in parallel. The pores run through from the part close to the bottom of the sample to the top of the sample. The sheets are filled with air. The specific surface area is large and the connectivity between the sheets is high. Material exchange and energy exchange with the external environment can be achieved. The reactant water molecules enter the pores to participate in the catalytic reaction, which can greatly increase the rate of hydrogen production by decomposing water.
[0039] The present invention uses ice as a pore-forming template to prepare a barium strontium titanate piezoelectric ceramic green body under low temperature and low pressure conditions, and obtains an oriented porous piezoelectric ceramic catalyst after high temperature sintering. The preparation method of the present invention is safe, environmentally friendly and low-cost. The oriented porous piezoelectric ceramic catalyst exhibits a high performance of decomposing water to produce hydrogen under ultrasonic vibration.
[0040] In a preferred embodiment, the hydrogen production rate of the porous oriented piezoelectric ceramic catalyst provided by the present invention is ≧400nmol / h. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 This is the XRD pattern of barium strontium titanate ceramic powder prepared by the method in Example 1.
[0042] Figure 2 This is the SEM image of the oriented porous piezoelectric ceramic catalyst prepared by the method in Example 1.
[0043] Figure 3 This is a comparison chart of the hydrogen production effects of the oriented porous piezoelectric ceramic catalysts prepared by the methods in Examples 1-3. DETAILED DESCRIPTION
[0044] Example 1
[0045] 26.8 g of strontium carbonate, 6.7 g of barium carbonate, 14.5 g of titanium dioxide and 70 ml were added to a ball mill, and the ceramic powder raw material suspension was obtained after ball milling for 24 hours; after the suspension was dried, the dried powder was placed in a muffle furnace, and the temperature was raised to 1200°C at 3°C / min, and the temperature was kept for 3 hours for solid phase reaction to obtain powder A; with alcohol as the medium, powder A was added to a ball mill, and powder B was obtained after planetary crushing for 48 hours; after drying powder B, it was sieved through 200 mesh and 400 mesh sieves to obtain barium strontium titanate ceramic powder.
[0046] In a 120 ml polypropylene bottle, add an appropriate amount of zirconium balls, 46.4 grams of strontium barium titanate ceramic powder, 12 ml of deionized water, and 0.464 grams of polyacrylate. After ball milling for 12 hours, add 4.64 grams of 5% polyvinyl alcohol aqueous solution. After mixing for 2 hours, pour the slurry into a mold, cool it to -90°C at a cooling rate of 10°C / min, freeze it for 20 minutes, demold the frozen sample, and dry the demolded sample at -50°C and 10 Pa. The dried green body is first heated to 600°C at 1°C / min to remove organic matter, and then heated to 1320°C at 3°C / min for sintering to obtain an oriented porous piezoelectric barium strontium titanate ceramic.
[0047] Figure 1 This is the XRD pattern of barium strontium titanate ceramic powder prepared by the method in Example 1. Figure 2 This is a SEM image of the oriented porous piezoelectric ceramic catalyst prepared by the method in Example 1. From the XRD image, it can be seen that the prepared powder phase is accurate; the SEM image shows that the piezoelectric ceramic catalyst with a lamellar oriented pore structure has been successfully prepared, the pores have good connectivity, the ceramic layer thickness is about 25μm, and the pore spacing is about 30μm.
[0048] After cutting barium strontium titanate ceramics, an oriented porous piezoelectric ceramic catalyst with a thickness of 1.5 mm and a porosity of 40% was obtained. It was placed in a closed reactor filled with 30 ml of pure water. Under ultrasonic conditions with a power of 80 watts, the rate of hydrogen production by decomposing water was 442 nmol / h.
[0049] Example 2
[0050] 26.8 g of strontium carbonate, 6.7 g of barium carbonate, 14.5 g of titanium dioxide and 70 ml were added to a ball mill, and the ceramic powder raw material suspension was obtained after ball milling for 24 hours; after the suspension was dried, the dried powder was placed in a muffle furnace, and the temperature was raised to 1200°C at 3°C / min, and the temperature was kept for 3 hours for solid phase reaction to obtain powder A; with alcohol as the medium, powder A was added to a ball mill, and powder B was obtained after planetary crushing for 48 hours; after drying powder B, it was sieved through 200 mesh and 400 mesh sieves to obtain barium strontium titanate ceramic powder.
[0051] In a 120 ml polypropylene bottle, add an appropriate amount of zirconium balls, 34.8 grams of strontium barium titanate ceramic powder, 12 ml of deionized water, and 0.464 grams of polyacrylate. After ball milling for 12 hours, add 3.48 grams of 5% polyvinyl alcohol aqueous solution. After mixing for 2 hours, pour the slurry into a mold, cool it to -90°C at a cooling rate of 10°C / min, freeze it for 20 minutes, demold the frozen sample, and dry the demolded sample at -50°C and 10 Pa. The dried green body is first heated to 600°C at 1°C / min to remove organic matter, and then heated to 1320°C at 3°C / min for sintering to obtain oriented porous piezoelectric barium strontium titanate ceramics.
[0052] After cutting barium strontium titanate ceramics, an oriented porous piezoelectric ceramic catalyst with a thickness of 1.5 mm and a porosity of 50% was obtained. It was placed in a closed reactor filled with 30 ml of pure water. Under ultrasonic conditions with a power of 80 watts, the rate of hydrogen production by decomposing water was 112 nmol / h.
[0053] Example 3
[0054] 26.8 g of strontium carbonate, 6.7 g of barium carbonate, 14.5 g of titanium dioxide and 70 ml were added to a ball mill, and the ceramic powder raw material suspension was obtained after ball milling for 24 hours; after the suspension was dried, the dried powder was placed in a muffle furnace, and the temperature was raised to 1200°C at 3°C / min, and the temperature was kept for 3 hours for solid phase reaction to obtain powder A; with alcohol as the medium, powder A was added to a ball mill, and powder B was obtained after planetary crushing for 48 hours; after drying powder B, it was sieved through 200 mesh and 400 mesh sieves to obtain barium strontium titanate ceramic powder.
[0055] In a 120 ml polypropylene bottle, add an appropriate amount of zirconium balls, 58 grams of strontium barium titanate ceramic powder, 12 ml of deionized water, and 0.464 grams of polyacrylate. After ball milling for 12 hours, add 5.8 grams of 5% polyvinyl alcohol aqueous solution by mass. After mixing for 2 hours, pour the slurry into a mold, cool it to -90°C at a cooling rate of 10°C / min, freeze it for 20 minutes, demold the frozen sample, and dry the demolded sample at -50°C and 10 Pa. The dried green body is first heated to 600°C at 1°C / min to remove organic matter, and then heated to 1320°C at 3°C / min for sintering to obtain oriented porous piezoelectric barium strontium titanate ceramics.
[0056] After cutting barium strontium titanate ceramics, an oriented porous piezoelectric ceramic catalyst with a thickness of 1.5 mm and a porosity of 30% was obtained. It was placed in a closed reactor filled with 30 ml of pure water. Under ultrasonic conditions with a power of 80 watts, the rate of hydrogen production by decomposing water was 237 nmol / h.
[0057] Comparative Example 1
[0058] The other conditions are the same as those in Example 1, except that 23.2 g of barium strontium titanate ceramic powder is added. The mechanical strength of the powder is not sufficient to support the test under ultrasonic conditions. The oriented porous piezoelectric ceramic catalyst will break under ultrasonic conditions, accompanied by the shedding of a large amount of ceramic powder, and the advantage of the recyclable porous piezoelectric ceramic catalyst cannot be achieved.
Claims
1. A method for preparing an oriented porous piezoelectric ceramic catalyst for catalytic decomposition of water to produce hydrogen, Features: The ceramic slurry is obtained by mixing the strontium barium titanate ceramic powder, water, a dispersant and a binder, and the ceramic slurry is placed in a mold, and then the mold is cooled to -90~-20°C at a cooling rate of 5~20°C / min, frozen for 15~30min, and then dried at -50~0°C and 1~100Pa to obtain a green body with an oriented porous structure, and the green body is sintered to obtain an oriented porous piezoelectric ceramic catalyst; In the ceramic slurry, the volume fraction of barium strontium titanate ceramic powder is 30 vol.% to 50 vol.%; The piezoelectric ceramic catalyst is an oriented porous structure, which is composed of ceramic sheets with a width of 10 to 80 μm and arranged in parallel, and the width of the pores between the ceramic sheets is 20 to 70 μm; The volume porosity of the oriented porous piezoelectric ceramic catalyst is 30-50%; The thickness of the oriented porous piezoelectric ceramic catalyst is 1-1.5 mm.
2. A method for preparing an oriented porous piezoelectric ceramic catalyst for catalytic decomposition of water to produce hydrogen according to claim 1, Features: The particle size of the barium strontium titanate ceramic powder is 1-3 μm.
3. A method for preparing an oriented porous piezoelectric ceramic catalyst for catalytic decomposition of water to produce hydrogen according to claim 1, Features: The preparation process of the barium strontium titanate ceramic powder is as follows: strontium carbonate, barium carbonate and titanium dioxide are prepared to obtain a mixed powder, the mixed powder is subjected to a first wet ball milling to obtain a suspension, the suspension is dried, and then a solid phase reaction is performed to obtain powder A, the powder A is subjected to a second wet ball milling to obtain powder B, and the powder B is dried and sieved to obtain the barium strontium titanate ceramic powder; In the mixed powder, in molar ratio, Ba: Sr: Ti: O = Ba: Sr: Ti: O = x: (1-x): 1: 3; The temperature of the solid phase reaction is 1200-1320°C, and the time of the solid phase reaction is 2-4h; The rotation speed of the second wet ball milling is 250-350 r / min, and the time of the second wet ball milling is 36-72 h.
4. The method for preparing an oriented porous piezoelectric ceramic catalyst for catalytic decomposition of water to produce hydrogen according to claim 1, Features: The dispersant is selected from at least one of ammonium citrate, tetramethylammonium hydroxide, ammonium polyacrylate, and polyacrylate; The adhesive is selected from at least one of polyvinyl alcohol, polyvinyl pyrrolidone, polyvinyl butyral, and carboxymethyl cellulose; The amount of the dispersant added is 0.5-2% of the mass of the barium strontium titanate ceramic powder; The amount of the adhesive added is 0.5-2% of the mass of the barium strontium titanate ceramic powder.
5. The method for preparing an oriented porous piezoelectric ceramic catalyst for catalytic decomposition of water to produce hydrogen according to claim 1, Features: The sintering process is to first increase the temperature to 550-650°C at a heating rate of 1-3°C / min and keep the temperature for 2-4 hours, and then increase the temperature to 1200-1320°C at a heating rate of 3-5°C / min and keep the temperature for 2-4 hours.
6. A method for preparing an oriented porous piezoelectric ceramic catalyst for catalytic decomposition of water to produce hydrogen according to claim 1, Features: The oriented porous piezoelectric ceramic catalyst has a hydrogen production rate of ≥100 nmol / h.
7. Use of an oriented porous piezoelectric ceramic catalyst for catalytic decomposition of water to produce hydrogen prepared by the preparation method according to any one of claims 1 to 6, Features: The oriented porous piezoelectric ceramic catalyst is used to catalyze water decomposition to produce hydrogen.