A low-temperature SCR catalyst and its preparation method and application

By growing layered metal hydroxides in situ on the support and calcining them to produce a low-temperature SCR catalyst, the problem of NOx removal in low-temperature flue gas in the non-electric industry is solved, the activity and efficiency of the catalyst is improved, and energy consumption and recovery costs are reduced.

CN115845907BActive Publication Date: 2024-11-29SICHUAN UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211626990.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2024-11-29
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently remove NOx in the non-electric industry flue gas under low temperature conditions, and the heating use of vanadium tungsten titanium catalysts will bring huge energy consumption and increase in recycling costs.

Method used

The precursor layered metal hydroxide is grown in situ on the support, and a low-temperature SCR catalyst is prepared by calcination. The support is a molecular sieve. The support is supported and bridged metal atoms form a layered metal oxide with a high specific surface area and uniform distribution, which is used in SCR catalysts. .

Benefits of technology

It realizes efficient conversion of NOx within the temperature window of 80-300°C, improves the active metal dispersion and catalytic efficiency of the catalyst, and reduces energy consumption and recovery costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115845907B_ABST
    Figure CN115845907B_ABST
Patent Text Reader

Abstract

The present invention discloses a low-temperature SCR catalyst and a preparation method and application thereof, belonging to the technical field of catalysts. The provided low-temperature SCR catalyst comprises a carrier molecular sieve and a layered metal oxide Mn-Cu loaded on the carrier molecular sieve by bridging metal atoms. The low-temperature SCR catalyst provided above uses a molecular sieve as a matrix and loads active metal Mn and Cu species in a manner of in-situ growth of a nano-sheet metal oxide precursor, thereby obtaining a low-temperature SCR catalyst with a high specific surface area, high dispersion of Mn and Cu species, and uniform distribution, which helps to further improve the catalytic efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalyst technology, and in particular to a low-temperature SCR catalyst and a preparation method and application thereof. Background Art

[0002] The current environment is facing serious air pollution problems represented by smog. Among the many precursors of smog, nitrogen oxides (NO x ) is an important one. NO x Large-scale emissions will not only cause acid rain, ozone layer damage and other problems, but also easily react with SO2, NH3 and hydrocarbon compounds in the atmosphere to form secondary particulate matter through complex chemical reactions, which will cause great harm to human health and the ecological environment. Flue gas denitrification in the non-power industry is the focus of my country's current atmospheric environmental governance work. The flue gas temperature is generally 80-300℃. Selective catalytic reduction (SCR) is currently the most effective method for removing NO x The most effective method. SCR technology uses NH3 as a reducing agent to convert NO x The core of the selective catalytic reduction technology is the catalyst. However, due to the low flue gas temperature (80-300°C) in the non-electricity industry, it is difficult to match the working temperature range (300-400°C) of the vanadium-tungsten-titanium catalyst in the thermal power industry. Direct heating will not only lead to huge energy consumption, but also the solid waste properties of vanadium species will increase the cost of catalyst recovery. Therefore, the development of efficient and stable low-temperature SCR catalysts is crucial to achieve NO reduction in flue gas in the non-electricity industry. x Effective governance is essential.

[0003] In view of the above problems, it is necessary to provide a low-temperature SCR catalyst and a preparation method and application thereof. Summary of the invention

[0004] The purpose of the present invention is to provide a low-temperature SCR catalyst and a preparation method and application thereof in order to overcome the defects of the above-mentioned prior art.

[0005] The present invention solves the technical problem by adopting the following technical solutions.

[0006] The invention provides a low-temperature SCR catalyst. The low-temperature SCR catalyst comprises a carrier and a layered metal oxide loaded on the carrier via bridging metal atoms.

[0007] The present invention also provides a method for preparing a low-temperature SCR catalyst, which comprises: in-situ growing a precursor layered metal hydroxide on a carrier, and then calcining to obtain a low-temperature SCR catalyst.

[0008] The present invention also provides a low temperature SCR catalyst for NO xFor conversion purposes, the low temperature window is 80-300°C.

[0009] The present invention has the following beneficial effects:

[0010] The present invention provides a low-temperature SCR catalyst and a preparation method and application thereof, wherein the low-temperature SCR catalyst comprises a carrier and a layered metal oxide loaded on the carrier by bridging metal atoms. The low-temperature SCR catalyst provided uses the carrier as a matrix, and loads active metals by in-situ growth of nano-sheet metal oxides by bridging metal atoms, thereby obtaining an SCR catalyst with a high specific surface area, high dispersion of active metals, and uniform distribution, which is conducive to further improving the catalytic efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0012] Figure 1 The scanning electron microscope images of the catalysts prepared in Example 1 and Comparative Example 1 are shown;

[0013] Figure 2 N2 adsorption-desorption curves of the catalysts prepared in Example 1 and Comparative Example 1;

[0014] Figure 3 Denitration efficiency curves of the catalysts at different temperatures were obtained for Example 1 and Comparative Example 1. DETAILED DESCRIPTION

[0015] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0016] The active components in low-temperature SCR catalysts are generally transition metal oxides (or metal ions), such as manganese oxides and copper oxides with good redox properties. Molecular sieves (Z) have the advantages of high specific surface area, regular and orderly pores, easy modification of active ions, and good thermal stability, and are widely used as SCR catalyst carriers. However, molecular sieve catalysts have the disadvantages of limited loading of active metal species (such as Mn and Cu) and difficulty in uniform distribution, which limits their multifunctional modification and further improvement of activity.

[0017] If a layered metal hydroxide (LDH) containing a target active metal (such as Mn, Cu) is prepared and then calcined, a target metal oxide (LDO)-based SCR catalyst can be obtained. The LDO catalyst prepared by this method can maintain the layered structure of LDH and has structural uniformity at the atomic level. Compared with conventional precipitation, impregnation and ion exchange methods, it is more conducive to the dispersion of active metal species on the denitrification catalyst. However, there are still some shortcomings in the current LDO catalyst: due to the aggregation and stacking of the layers, the specific surface area is small, which hinders the contact between the reactants and the active components and is not conducive to further improving the catalytic efficiency. If the molecular sieve can be used as the matrix and the active metal Mn and Cu species can be loaded by in-situ growth of nanosheet metal oxide precursors, it is expected to obtain an LDO / Z catalyst with a high specific surface area, high dispersion of Mn and Cu atoms, and uniform distribution, which will help to further improve the catalytic efficiency.

[0018] A low-temperature SCR catalyst, a preparation method and an application thereof provided in an embodiment of the present invention are described in detail below.

[0019] In a first aspect, an embodiment of the present invention provides a low-temperature SCR catalyst, which includes a carrier and a layered metal oxide supported on the carrier via bridging metal atoms.

[0020] In an alternative embodiment, the bridging metal atom is Al, and the layered metal oxide is a layered metal oxide of Mn and / or Cu and Al, wherein the bridging metal atom forms at least one covalent bond with each adjacent support and layered metal oxide.

[0021] In an optional embodiment, the molar ratio of Al, Mn and / or Cu in the low temperature SCR catalyst is 0.8-1.2:1.5-2.5.

[0022] In an optional embodiment, the layered metal oxide accounts for 40-60% of the low temperature SCR catalyst.

[0023] In an optional embodiment, the carrier is a molecular sieve, and the molecular sieve includes any one of NaY, ZSM-5, 13X, MCM-41, SBA-15, USY, MOR, SSZ-13, SAPO-34, and SSZ-39.

[0024] In a second aspect, an embodiment of the present invention further provides a method for preparing a low-temperature SCR catalyst, which comprises: in-situ growing a precursor layered metal hydroxide on a carrier, and then calcining to obtain a low-temperature SCR catalyst.

[0025] In an optional embodiment, the steps include: dissolving manganese salt or copper salt, aluminum salt in water to obtain a first solution, dissolving molecular sieve and carbonate in water to obtain a second solution, continuously stirring the second solution, and then slowly dropping the first solution into the second solution, using alkaline solution to adjust the pH of the solution during the dropping process, continuously stirring after the dropping is completed, standing for aging, and then filtering, washing and drying the mixed solution to obtain a carrier-loaded precursor layered metal hydroxide powder, and calcining the obtained powder under high temperature conditions to obtain a low-temperature SCR catalyst.

[0026] In an optional embodiment, the manganese salt is manganese chloride, manganese nitrate or manganese sulfate; the aluminum salt is aluminum chloride, aluminum nitrate or aluminum sulfate; the copper salt is copper chloride, copper nitrate or copper sulfate; the carbonate is sodium carbonate or potassium carbonate, and the alkali solution is sodium hydroxide;

[0027] Preferably, the rate of dripping the first solution into the second solution is 0.01-0.5 mL / min, and the pH of the solution is adjusted to 9-11 using alkaline solution; and the aging time is 1-48 h.

[0028] In an optional embodiment, the mixed solution is filtered and washed, dried at 50-100° C., and then calcined at 300-600° C. for 1-6 hours to obtain a low-temperature SCR catalyst.

[0029] In a third aspect, the present invention also provides a low-temperature SCR catalyst for NO in a low temperature window. x For conversion purposes, the low temperature window is 80-300°C.

[0030] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0031] Example 1

[0032] 1. Weigh 1.09ml of 50% Mn(NO3)2 solution, 1.79g Al(NO3)3·9H2O and 2.32g Cu(NO3)2 and dissolve them in 200ml deionized water, marked as solution A. At the same time, weigh 2g Na-Y zeolite and 1.06g NaCO3 and dissolve them in 200ml deionized water, marked as solution B. Stir solution B continuously and add solution A slowly, adjusting pH while adding. Stir continuously for 2h after adding and let stand for 24h. After standing, filter and wash until neutral, dry at 105℃ and calcine at 500℃ in air atmosphere for 4h. Sample number is 1.

[0033] The preparation method of sample No. 2-7 prepared in Example 2-7 is similar to that of sample No. 1. The specific amounts used are shown in Table 1.

[0034] Comparative Example 1

[0035] Prepared by impregnation method: 1.09ml 50% Mn(NO3)2 solution, 1.79g Al(NO3)3·9H2O and 2.32g Cu(NO3)2 were dissolved in 200ml deionized water. After sufficient stirring, 2g Na-Y zeolite was poured in. After sufficient standing, it was placed in an oven at 80℃ for drying, and then calcined at 500℃ for 4h in air. Sample number is 8.

[0036] Comparative Example 2

[0037] The steps are similar to those in Example 1, except that the salt solutions used are copper nitrate, iron nitrate, and aluminum nitrate, and the sample number is 9.

[0038] Comparative Example 3

[0039] The steps are similar to those in Example 1, except that the salt solutions used are copper nitrate, cerium nitrate, and aluminum nitrate, and the sample number is 10.

[0040] Comparative Example 4

[0041] The steps are similar to those of Example 1, except that solution B is continuously stirred and directly poured into solution A to mix with the solution B. Sample number is 11.

[0042] Test results:

[0043] The SEM images of the catalysts obtained in Example 1 and Comparative Example 1 are shown in Figure 1 It can be seen that the catalyst prepared in Example 1 presents an obvious lamellar structure, which is more conducive to the dispersion of active species (metal oxides). Figure 2 It can be seen that compared with Comparative Example 1, the catalyst prepared in Example 1 has a larger specific surface area (374m 2 / g), which is more conducive to the contact between the reactants and the catalyst, thereby promoting the SCR reaction and obtaining better catalytic efficiency.

[0044] Catalyst denitrification activity test method:

[0045] In order to compare and illustrate the properties of the catalysts of different embodiments and comparative examples, the denitration activities of the catalysts of embodiments 1-8 were tested. The test results are shown in Table 1.

[0046] The denitrification activity test method of the denitrification catalyst is as follows: the experimental flue gas is simulated by a mixed gas cylinder. The flue gas components include NO, O2, N2 (balance gas) and SO2 (if used). The gas is mixed in the mixer after the flow rate is controlled by a mass flow meter. The gas is carried out in a tubular reactor with an inner diameter of about 1.5 cm. The catalyst is located in the middle of the reactor. The prepared simulated flue gas and the NH3 directly entering the tubular reactor undergo redox reactions on the catalyst. The reacted gas first passes through a phosphoric acid absorption bottle to remove NH3 that does not participate in the reaction, and then passes through an anti-backflow bottle (condensation bottle). The detection system consists of a display and an online infrared flue gas analyzer to detect the concentrations of NO, O2 and SO2 (if used) at the inlet and outlet of the reaction system. The tail gas treatment system absorbs the NO and SO2 (if used) detected by the online infrared flue gas analyzer through alkali solution to avoid pollution to the external atmospheric environment.

[0047] The simulated flue gas composition for denitrification activity test is: 536mg / m 3 NO, 304mg / m 3 NH3 (i.e., the volume ratio of ammonia nitrogen is NH3:NO = 1:1), 5% O2, with N2 as the balance gas, the total gas flow rate is 900mL / min, and the gas space velocity (GHSV) is 45000h -1 The concentrations of NO and O2 at the inlet and outlet of the reaction system were detected by the GAS-board3000 online infrared flue gas analyzer of Wuhan Sifang Optoelectronics Technology Co., Ltd. The activity test temperature range was 100-300°C. The test results of the catalyst denitrification activity were evaluated by the conversion rate of NO, and the calculation formula is shown in formula (1):

[0048]

[0049] In the above formula, NO conversion (%) is NO x The conversion rate of NO in and NO out is the inlet and outlet concentration of NO (mg / m 3 ).

[0050] Table 1

[0051]

[0052]

[0053] Combining Table 1 and Figure 3 , the results of the embodiments of the present invention and the comparative examples are analyzed, and the following conclusions can be drawn: the denitration effect is good, especially the low-temperature denitration activity is excellent. When the temperature is 175°C and the air velocity is high (45000h -1), the denitration efficiency is as high as 97.1%. At 150°C, the denitration efficiency can also reach 95.8%, which is far beyond the reach of Comparative Example 1 (the denitration efficiency is only 34.0% and 52.8% at 150°C and 175°C).

[0054] In summary, the embodiments of the present invention provide a low-temperature SCR catalyst and a preparation method and application thereof. The low-temperature SCR catalyst includes a carrier molecular sieve and a layered metal oxide Mn-Cu loaded on the carrier molecular sieve through bridging metal atoms. The low-temperature SCR catalyst provided above uses a molecular sieve as a matrix and loads active metal Mn and Cu species by in-situ growing a nanosheet metal oxide precursor, thereby obtaining a low-temperature SCR catalyst with a high specific surface area, high dispersion of Mn and Cu species, and uniform distribution, which helps to further improve the catalytic efficiency.

[0055] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a low-temperature SCR catalyst, characterized in that: The method comprises the following steps: weighing 1.09 ml of 50% Mn(NO3)2 solution, 1.79 g of Al(NO3)3·9H2O and 2.32 g of Cu(NO3)2 and dissolving them in 200 ml of deionized water, which is marked as solution A; weighing 2 g of Na-Y zeolite and 1.06 g of Na2CO3 and dissolving them in 200 ml of deionized water, which is marked as solution B; stirring the solution B continuously and slowly adding the solution A while adjusting the pH value during the dropwise addition; stirring continuously for 2 hours after the dropwise addition is completed and allowing the catalyst to stand for 24 hours; filtering and washing the catalyst to neutrality after allowing the catalyst to stand for 24 hours, drying the catalyst at 105°C and calcining the catalyst at 500°C in an air atmosphere for 4 hours, and the low temperature window of the prepared low-temperature SCR catalyst is 80-300°C.

2. A method for preparing a low-temperature SCR catalyst, characterized in that: The method comprises the following steps: weighing 1.09 ml of 50% Mn(NO3)2 solution, 1.79 g of Al(NO3)3·9H2O and 2.32 g of Cu(NO3)2 and dissolving them in 200 ml of deionized water, which is marked as solution A; weighing 2 g of 13X and 1.06 g of Na2CO3 and dissolving them in 200 ml of deionized water, which is marked as solution B; stirring the solution B continuously and slowly adding the solution A while adjusting the pH value during the dropwise addition; stirring continuously for 2 hours after the dropwise addition is completed and allowing the catalyst to stand for 24 hours; filtering and washing the catalyst to neutrality after allowing the catalyst to stand for 24 hours, drying the catalyst at 105°C and calcining the catalyst at 500°C in an air atmosphere for 4 hours, wherein the low temperature window of the prepared low-temperature SCR catalyst is 80-300°C.

Citation Information

Patent Citations

  • Denitration sulfur-resistant catalyst with core-shell structure as well as preparation method and application of denitration sulfur-resistant catalyst

    CN114653397A