Tungsten carbide-cobalt reinforced copper-based composite coating, tungsten carbide-cobalt reinforced copper-based composite coating and preparation method thereof

The preparation of tungsten carbide-cobalt reinforced copper-based composite coating by cold spraying method of using tungsten carbide-cobalt composite powder and copper powder on the copper-based metal surface, and the problems of poor density and low bonding strength of traditional coatings are solved, and the problem of Efficient friction and wear resistance.

CN115846657BActive Publication Date: 2024-12-03TAIZHOU HUIMO TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211659780.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-23
Publication Date
2024-12-03
Estimated Expiration
2042-12-23

AI Technical Summary

Technical Problem

In the traditional copper-based metal cermet composite coating preparation process, the temperature is high and the density is poor, resulting in low bonding strength and the hard particles of tungsten carbide ceramics are prone to fall off, reducing friction and wear resistance.

Method used

The tungsten carbide-cobalt reinforced copper-based composite coating was prepared by cold spraying method of tungsten carbide-cobalt composite powder and copper powder. The cobalt metal layer was formed through chemical activation and electroless plating treatment, which improved the bonding performance and maintained by cold spraying method. The powder coated state enhances density and wear resistance.

Benefits of technology

The good density and excellent friction and wear resistance of the tungsten carbide-cobalt reinforced copper-based composite coating are achieved, with a friction coefficient of 0.59~0.65 and a wear rate of 8.95~10.3 (10-2mm3·N-1·m-1), Significantly improves friction and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115846657B_ABST
    Figure CN115846657B_ABST
Patent Text Reader

Abstract

The present invention provides a tungsten carbide-cobalt reinforced copper-based composite coating, a tungsten carbide-cobalt reinforced copper-based composite coating and a preparation method, and relates to the technical field of metal-based ceramic composite coating preparation. The tungsten carbide-cobalt reinforced copper-based composite coating provided by the present invention comprises a tungsten carbide-cobalt composite powder and copper powder; the tungsten carbide-cobalt composite powder comprises a tungsten carbide powder and a cobalt metal layer coated on the surface of the tungsten carbide powder. The present invention adopts a compound of tungsten carbide-cobalt composite powder and copper powder. Since metal cobalt and metal copper have good wettability, the tungsten carbide-cobalt reinforced copper-based composite coating prepared by using the tungsten carbide-cobalt composite powder has good density and excellent friction and wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of metal-based ceramic composite coatings, and specifically relates to a tungsten carbide-cobalt reinforced copper-based composite coating, a tungsten carbide-cobalt reinforced copper-based composite coating and a preparation method thereof. Background Art

[0002] In order to improve the friction and wear resistance of metallic copper and copper alloys, tungsten carbide (WC) ceramic hard particles are usually doped into copper and copper alloys to prepare copper-based metal-ceramic composite coatings. Traditional copper-based metal-ceramic composite coatings are deposited by thermal spraying processes such as laser cladding, plasma spraying, and high-oxygen fuel spraying. These process methods have high preparation temperatures, usually exceeding 1500°C, and are prone to forming brittle intermetallic phases, severe oxidation, and poor density.

[0003] At the same time, in the copper-based metal-ceramic composite coating prepared by thermal spraying processes such as laser cladding, plasma spraying, and high-oxygen fuel spraying, the bonding strength between the metal substrate and the WC ceramic hard particles is low. During the wear process, the WC ceramic hard particles are easily fallen off from the surface of the metal substrate, resulting in abrasive wear of the copper-based metal-ceramic composite coating, accelerating the wear failure of the copper-based metal-ceramic composite coating and reducing the friction and wear resistance. Summary of the invention

[0004] The purpose of the present invention is to provide a tungsten carbide-cobalt reinforced copper-based composite coating, a tungsten carbide-cobalt reinforced copper-based composite coating and a preparation method. The tungsten carbide-cobalt reinforced copper-based composite coating prepared by using the tungsten carbide-cobalt reinforced copper-based composite coating provided by the present invention has good density and excellent friction and wear resistance.

[0005] In order to achieve the purpose of the present invention, the present invention provides the following technical solutions:

[0006] A tungsten carbide-cobalt reinforced copper-based composite coating comprises a tungsten carbide-cobalt composite powder and copper powder; the tungsten carbide-cobalt composite powder comprises a tungsten carbide powder and a cobalt metal layer coated on the surface of the tungsten carbide powder.

[0007] Preferably, the mass ratio of the tungsten carbide-cobalt composite powder to the copper powder is 1:9 to 2:3.

[0008] Preferably, the mass fraction of cobalt in the tungsten carbide-cobalt composite powder is 5-15%.

[0009] The present invention also provides a method for preparing the tungsten carbide-cobalt reinforced copper-based composite coating described in the above technical solution, comprising the following steps:

[0010] Mixing tungsten carbide powder with chemical activation liquid and performing activation treatment to obtain activated tungsten carbide powder;

[0011] The activated tungsten carbide powder is mixed with a cobalt-containing chemical plating solution, and a cobalt metal layer is formed on the surface of the activated tungsten carbide powder through chemical plating to obtain a tungsten carbide-cobalt composite powder;

[0012] The tungsten carbide-cobalt composite powder and copper powder are mixed to obtain a tungsten carbide-cobalt reinforced copper-based composite coating.

[0013] Preferably, the chemical activation solution comprises hydrofluoric acid, nitric acid, ammonium fluoride and water; the content of hydrofluoric acid in the chemical activation solution is 20-40 mL / L, the content of nitric acid is 30-60 mL / L, and the content of ammonium fluoride is 2-5 g / L; the concentration of the hydrofluoric acid is 40 wt %, and the concentration of the nitric acid is 98 wt %.

[0014] Preferably, the cobalt-containing chemical plating solution comprises cobalt sulfate, sodium hypophosphite, trisodium citrate, boric acid and water; the content of cobalt sulfate in the cobalt-containing chemical plating solution is 20-30 g / L, the content of sodium hypophosphite is 20-30 g / L, the content of trisodium citrate is 40-60 g / L, and the content of boric acid is 20-30 g / L; the pH value of the cobalt-containing chemical plating solution is 9-11.

[0015] Preferably, the average particle size of the tungsten carbide powder is 5 to 30 μm; the average particle size of the tungsten carbide-cobalt composite powder is 5 to 32 μm; and the average particle size of the copper powder is 10 to 40 μm.

[0016] The present invention also provides a method for preparing the tungsten carbide-cobalt reinforced copper-based composite coating described in the above technical scheme, comprising the following steps: spraying the tungsten carbide-cobalt reinforced copper-based composite coating onto the surface of a metal substrate by a cold spraying method, thereby obtaining a tungsten carbide-cobalt reinforced copper-based composite coating on the surface of the metal substrate; the tungsten carbide-cobalt reinforced copper-based composite coating is the tungsten carbide-cobalt reinforced copper-based composite coating described in the above technical scheme or the tungsten carbide-cobalt reinforced copper-based composite coating prepared by the preparation method described in the above technical scheme.

[0017] Preferably, the operating conditions of the cold spraying method include: the carrier gas is nitrogen; the spraying temperature is 500-700° C.; the spraying pressure is 2.5-5 MPa; and the spraying distance is 20-40 mm.

[0018] The present invention also provides a tungsten carbide-cobalt reinforced copper-based composite coating prepared by the above preparation method, comprising a copper-based layer, tungsten carbide particles doped in the copper-based layer, and a cobalt metal layer located between the copper-based layer and the tungsten carbide.

[0019] The present invention provides a tungsten carbide-cobalt reinforced copper-based composite coating, comprising a tungsten carbide-cobalt composite powder and copper powder; the tungsten carbide-cobalt composite powder comprises a tungsten carbide powder and a cobalt metal layer coated on the surface of the tungsten carbide powder. The present invention uses a tungsten carbide-cobalt composite powder and a copper powder for compounding. Since metal cobalt and metal copper have good wettability, the tungsten carbide-cobalt reinforced copper-based composite coating prepared by using the tungsten carbide-cobalt composite powder has good compactness, and in the process of friction and wear, the tungsten carbide-cobalt composite powder can be well pinned in the copper base layer, significantly improving the bonding performance between the metal matrix and the ceramic particles, thereby improving the friction and wear resistance of the tungsten carbide-cobalt reinforced copper-based composite coating.

[0020] At the same time, the present invention adopts a cold spraying method to prepare a tungsten carbide-cobalt reinforced copper-based composite coating. During the cold spraying preparation process, the tungsten carbide-cobalt composite powder can still maintain the coated state of the original powder, which is conducive to obtaining a tungsten carbide-cobalt reinforced copper-based composite coating with a dense structure and excellent friction and wear resistance.

[0021] The experimental results show that the tungsten carbide-cobalt reinforced copper-based composite coating prepared by the present invention has good compactness; at the same time, the friction coefficient of the tungsten carbide-cobalt reinforced copper-based composite coating prepared by the present invention is 0.59-0.65, and the wear rate is 8.95-10.3 (10 -2 mm 3 ·N -1 ·m -1 ), excellent friction and wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0023] Figure 1 This is a cross-sectional SEM image of the tungsten carbide-cobalt composite powder prepared in Example 1;

[0024] Figure 2 This is a cross-sectional SEM image of the tungsten carbide-cobalt reinforced copper-based composite coating prepared in Example 1;

[0025] Figure 3 This is a partial enlarged cross-sectional SEM image of the tungsten carbide-cobalt reinforced copper-based composite coating prepared in Example 1;

[0026] Figure 4 This is a friction and wear morphology of the tungsten carbide-cobalt reinforced copper-based composite coating prepared in Example 1;

[0027] Figure 5 This is a friction coefficient curve of the tungsten carbide-cobalt reinforced copper-based composite coating prepared in Example 1;

[0028] Figure 6 This is the friction and wear morphology of the copper coating prepared in Comparative Example 1;

[0029] Figure 7 The friction coefficient curve of the copper coating prepared in Comparative Example 1;

[0030] Figure 8 This is a friction and wear morphology of the tungsten carbide reinforced copper-based composite coating prepared in Comparative Example 2;

[0031] Fig. 9 This is a friction coefficient curve of the tungsten carbide reinforced copper-based composite coating prepared in Comparative Example 2. DETAILED DESCRIPTION

[0032] The invention provides a tungsten carbide-cobalt reinforced copper-based composite coating, comprising a tungsten carbide-cobalt composite powder and copper powder; the tungsten carbide-cobalt composite powder comprises a tungsten carbide powder and a cobalt metal layer coated on the surface of the tungsten carbide powder.

[0033] The tungsten carbide-cobalt reinforced copper-based composite coating provided by the present invention comprises a tungsten carbide-cobalt composite powder, and the average particle size of the tungsten carbide-cobalt composite powder is preferably 5 to 32 μm, and more preferably 20 μm. In the present invention, the tungsten carbide-cobalt composite powder comprises a tungsten carbide powder and a cobalt metal layer coated on the surface of the tungsten carbide powder, and the mass fraction of cobalt in the tungsten carbide-cobalt composite powder is preferably 5 to 15%, and more preferably 10%.

[0034] The tungsten carbide-cobalt reinforced copper-based composite coating provided by the present invention comprises copper powder, and the average particle size of the copper powder is preferably 10 to 40 μm, more preferably 20 μm.

[0035] In the present invention, the mass ratio of the tungsten carbide-cobalt composite powder to the copper powder is preferably 1:9 to 2:3, and more preferably 1:4 to 3:7.

[0036] The present invention also provides a method for preparing the tungsten carbide-cobalt reinforced copper-based composite coating described in the above technical solution, comprising the following steps:

[0037] Mixing tungsten carbide powder with chemical activation liquid and performing activation treatment to obtain activated tungsten carbide powder;

[0038] The activated tungsten carbide powder is mixed with a cobalt-containing chemical plating solution, and a cobalt metal layer is formed on the surface of the activated tungsten carbide powder through chemical plating to obtain a tungsten carbide-cobalt composite powder;

[0039] The tungsten carbide-cobalt composite powder and copper powder are mixed to obtain a tungsten carbide-cobalt reinforced copper-based composite coating.

[0040] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known to those skilled in the art.

[0041] The present invention mixes tungsten carbide powder with a chemical activation liquid, performs activation treatment, and obtains activated tungsten carbide powder. In the present invention, the average particle size of the tungsten carbide powder is preferably 5 to 30 μm, and more preferably 20 μm. In the present invention, the chemical activation liquid preferably includes hydrofluoric acid, nitric acid, ammonium fluoride and water; the content of hydrofluoric acid in the chemical activation liquid is preferably 20 to 40 mL / L, more preferably 25 to 35 mL / L, and further preferably 30 mL / L; the content of nitric acid is preferably 30 to 60 mL / L, more preferably 40 to 50 mL / L; the content of ammonium fluoride is preferably 2 to 5 g / L, more preferably 3 to 4 g / L; the concentration of hydrofluoric acid is preferably 40 wt%; the concentration of nitric acid is 98 wt%. In the present invention, the water is preferably deionized water.

[0042] The present invention has no particular limitation on the mixing method of the tungsten carbide powder and the chemical activation solution, and any method well known to those skilled in the art may be used.

[0043] In the present invention, the solid-liquid ratio of the tungsten carbide powder to the chemical activation solution is preferably 30 to 100 g / L, more preferably 40 to 50 g / L.

[0044] In the present invention, the temperature of the activation treatment is preferably 10-35°C, more preferably 25°C; the time of the activation treatment is preferably 20-40min, more preferably 30min. In the present invention, the activation treatment is preferably carried out under ultrasonic and stirring conditions. In the present invention, the power of the ultrasound is preferably 300-400W; the stirring rate is preferably 100-300r / min. In the present invention, the activation treatment can produce a large number of crystal defects on the surface of the tungsten carbide powder, which is conducive to obtaining a cobalt metal layer on the surface of the tungsten carbide powder by chemical plating.

[0045] In the present invention, after the activation treatment, it is preferred that the activation treatment further comprises: placing the obtained liquid after the activation treatment for static sedimentation, and then subjecting the obtained solid material to solid-liquid separation, washing the obtained solid material to obtain activated tungsten carbide powder. The present invention does not specifically limit the solid-liquid separation method, and a method well known to those skilled in the art can be used, such as filtering. In the present invention, the washing is preferably performed 3 times with deionized water. The present invention does not specifically limit the washing method, and a method well known to those skilled in the art can be used.

[0046] After obtaining the activated tungsten carbide powder, the present invention mixes the activated tungsten carbide powder with a cobalt-containing chemical plating solution, and forms a cobalt metal layer on the surface of the activated tungsten carbide powder through chemical plating treatment to obtain a tungsten carbide-cobalt composite powder. In the present invention, the cobalt-containing chemical plating solution preferably includes cobalt sulfate, sodium hypophosphite, trisodium citrate, boric acid and water. In the present invention, the content of cobalt sulfate in the cobalt-containing chemical plating solution is preferably 20-30 g / L, more preferably 25 g / L; the content of sodium hypophosphite is preferably 20-30 g / L, more preferably 25 g / L; the content of trisodium citrate is preferably 40-60 g / L, more preferably 50 g / L; the content of boric acid is preferably 20-30 g / L, more preferably 25 g / L.

[0047] In the present invention, the pH value of the cobalt-containing chemical plating solution is preferably 9-11, more preferably 10; the present invention preferably uses an alkaline agent to adjust the pH value of the cobalt-containing chemical plating solution to 9-11, and the alkaline agent is preferably sodium hydroxide.

[0048] In the present invention, the solid-to-liquid ratio of the activated tungsten carbide powder to the cobalt-containing chemical plating solution is preferably 30 to 100 g / L, more preferably 30 to 50 g / L.

[0049] In the present invention, the conditions for the chemical plating treatment preferably include: the chemical plating temperature is preferably 70 to 90° C., more preferably 80° C., and the chemical plating treatment time is preferably 1 to 2 hours, more preferably 1.5 hours.

[0050] In the present invention, the chemical plating treatment preferably further comprises: placing the obtained liquid after the chemical plating treatment for static sedimentation, and then subjecting the obtained solid material to solid-liquid separation, and washing the obtained solid material to obtain a tungsten carbide-cobalt composite powder. The present invention does not specifically limit the solid-liquid separation method, and a method well known to those skilled in the art can be used, such as filtering. In the present invention, the washing is preferably performed 3 times with deionized water. The present invention does not specifically limit the washing method, and a method well known to those skilled in the art can be used.

[0051] After obtaining the tungsten carbide-cobalt composite powder, the present invention mixes the tungsten carbide-cobalt composite powder with copper powder to obtain a tungsten carbide-cobalt reinforced copper-based composite coating. The present invention preferably uses a powder mixer to mix the tungsten carbide-cobalt composite powder with copper powder.

[0052] The present invention also provides a method for preparing the tungsten carbide-cobalt reinforced copper-based composite coating described in the above technical solution, comprising the following steps:

[0053] The tungsten carbide-cobalt reinforced copper-based composite coating is sprayed onto the surface of a metal substrate by a cold spraying method, so as to obtain a tungsten carbide-cobalt reinforced copper-based composite coating on the surface of the metal substrate; the tungsten carbide-cobalt reinforced copper-based composite coating is the tungsten carbide-cobalt reinforced copper-based composite coating described in the above technical scheme or the tungsten carbide-cobalt reinforced copper-based composite coating prepared by the preparation method described in the above technical scheme.

[0054] In the present invention, the metal substrate is preferably one of a copper substrate, an aluminum substrate, a magnesium substrate and a titanium substrate, and is more preferably an aluminum substrate.

[0055] In the present invention, the conditions of the cold spraying method preferably include: the carrier gas is preferably nitrogen; the spraying temperature is preferably 500-700°C, more preferably 600-650°C; the spraying pressure is preferably 2.5-5MPa, more preferably 3-4MPa; the spraying distance is preferably 20-40mm, more preferably 25-30mm.

[0056] In the present invention, the process of sandblasting and cleaning the metal substrate surface is preferably performed before spraying. The present invention does not specifically limit the specific operation method of sandblasting, and a method well known to those skilled in the art can be used. In the present invention, the cleaning agent is preferably alcohol; and the cleaning is preferably performed under ultrasonic conditions.

[0057] The present invention also provides a tungsten carbide-cobalt reinforced copper-based composite coating prepared by the preparation method described in the above technical solution, comprising a copper-based layer, tungsten carbide particles doped in the copper-based layer, and a cobalt metal layer located between the copper-based layer and the tungsten carbide.

[0058] In the present invention, the thickness of the tungsten carbide-cobalt reinforced copper-based composite coating is preferably 200-1000 μm, more preferably 300-700 μm, and further preferably 400-500 μm.

[0059] In order to further illustrate the present invention, the tungsten carbide-cobalt reinforced copper-based composite coating provided by the present invention is described in detail below in conjunction with the accompanying drawings and examples, but they should not be construed as limiting the protection scope of the present invention.

[0060] Example 1

[0061] Mix 30 mL of 40 wt % hydrofluoric acid, 50 mL of 98 wt % nitric acid, 3 g of ammonium chloride and 1 L of deionized water to prepare a chemical activation solution;

[0062] 50 g of cobalt sulfate, 50 g of sodium hypophosphite, 100 g of trisodium citrate, 50 g of boric acid and 2 L of deionized water were mixed, and the pH value was adjusted to 10 with sodium hydroxide to prepare a cobalt-containing chemical plating solution;

[0063] Weigh 50g of WC powder with an average particle size of 20μm and mix it with 1L of the chemical activation solution, perform activation treatment for 30min under the conditions of ultrasonic power of 350W and stirring rate of 200r / min, let it stand for sedimentation and filter to separate, and obtain filter residue; wash it with deionized water for 3 times to obtain activated tungsten carbide powder;

[0064] Weigh 30 g of the activated tungsten carbide powder and mix it with 1 L of the cobalt-containing chemical plating solution, perform chemical plating for 1.5 h at 80 ° C, an ultrasonic power of 350 W and a stirring rate of 200 r / min, and form a cobalt metal layer on the surface of the activated tungsten carbide powder. Then, let it stand and settle, filter and separate to obtain a filter residue; wash it with deionized water 3 times to obtain 33 g of tungsten carbide-cobalt composite powder;

[0065] Weigh 10 g of the tungsten carbide-cobalt composite powder and 40 g of copper powder with an average particle size of 20 μm, and mix them evenly using a powder mixer to obtain a tungsten carbide-cobalt reinforced copper-based composite coating;

[0066] The aluminum metal substrate is subjected to sandblasting treatment, and then cleaned with alcohol under ultrasonic conditions to obtain a pretreated aluminum metal substrate;

[0067] Weigh 20 g of the tungsten carbide-cobalt reinforced copper-based composite coating, and use a cold spray method to spray the tungsten carbide-cobalt reinforced copper-based composite coating onto the surface of a pretreated aluminum metal substrate to obtain a tungsten carbide-cobalt reinforced copper-based composite coating with a thickness of 500 μm; wherein the conditions of the cold spray method are: the carrier gas is nitrogen; the spraying temperature is 650°C; the spraying pressure is 3.5 MPa; and the spraying distance is 30 mm.

[0068] Example 2

[0069] Mix 30 mL of 40 wt % hydrofluoric acid, 50 mL of 98 wt % nitric acid, 3 g of ammonium chloride and 1 L of deionized water to prepare a chemical activation solution;

[0070] 50 g of cobalt sulfate, 50 g of sodium hypophosphite, 100 g of trisodium citrate, 50 g of boric acid and 2 L of deionized water were mixed, and the pH value was adjusted to 10 with sodium hydroxide to prepare a cobalt-containing chemical plating solution;

[0071] Weigh 50g of WC powder with an average particle size of 20μm and mix it with 1L of the chemical activation solution, perform activation treatment for 30min under the conditions of ultrasonic power of 350W and stirring rate of 200r / min, let it stand for sedimentation and filter to separate, and obtain filter residue; wash it with deionized water for 3 times to obtain activated tungsten carbide powder;

[0072] Weigh 30 g of the activated tungsten carbide powder and mix it with the cobalt-containing chemical plating solution, perform chemical plating for 1.5 h at 80° C., an ultrasonic power of 350 W, and a stirring rate of 200 r / min, to form a cobalt metal layer on the surface of the activated tungsten carbide powder, and then let it stand for sedimentation and filter to obtain a filter residue; wash it with deionized water 3 times to obtain 33 g of tungsten carbide-cobalt composite powder;

[0073] Weigh 12.5 g of the tungsten carbide-cobalt composite powder and 37.5 g of copper powder with an average particle size of 20 μm, and mix them evenly using a powder mixer to obtain a tungsten carbide-cobalt reinforced copper-based composite coating;

[0074] The aluminum metal substrate is subjected to sandblasting treatment, and then cleaned with alcohol under ultrasonic conditions to obtain a pretreated aluminum metal substrate;

[0075] Weigh 50 g of the tungsten carbide-cobalt reinforced copper-based composite coating, and use a cold spray method to spray the tungsten carbide-cobalt reinforced copper-based composite coating onto the surface of a pretreated aluminum metal substrate to obtain a tungsten carbide-cobalt reinforced copper-based composite coating with a thickness of 500 μm; wherein the conditions of the cold spray method are: the carrier gas is nitrogen; the spraying temperature is 650°C; the spraying pressure is 3.5 MPa; and the spraying distance is 30 mm.

[0076] Comparative Example 1

[0077] The aluminum metal substrate is subjected to sandblasting treatment, and then cleaned with alcohol under ultrasonic conditions to obtain a pretreated aluminum metal substrate;

[0078] 50 g of copper powder with an average particle size of 20 μm was weighed, and the copper powder was sprayed onto the surface of a pretreated aluminum metal substrate by a cold spraying method to obtain a copper coating with a thickness of 500 μm; wherein the conditions of the cold spraying method were: the carrier gas was nitrogen; the spraying temperature was 650° C.; the spraying pressure was 3.5 MPa; and the spraying distance was 30 mm.

[0079] Comparative Example 2

[0080] Weigh 10 g of tungsten carbide powder with an average particle size of 20 μm and 40 g of copper powder with an average particle size of 20 μm, and mix them evenly using a powder mixer to obtain a mixed powder;

[0081] The aluminum metal substrate is subjected to sandblasting treatment, and then cleaned with alcohol under ultrasonic conditions to obtain a pretreated aluminum metal substrate;

[0082] Weigh 50 g of the mixed powder and spray the mixed powder onto the surface of a pretreated aluminum metal substrate using a cold spray method to obtain a tungsten carbide reinforced copper-based composite coating with a thickness of 500 μm; wherein the conditions of the cold spray method are: the carrier gas is nitrogen; the spraying temperature is 650°C; the spraying pressure is 3.5 MPa; and the spraying distance is 30 mm.

[0083] Test Example 1

[0084] The tungsten carbide-cobalt composite powder and the tungsten carbide-cobalt reinforced copper-based composite coating prepared in Example 1 were characterized. Figures 1 to 3 shown.

[0085] Depend on Figure 1 It can be seen that the tungsten carbide-cobalt composite powder prepared in Example 1 has a core-shell structure, the core is tungsten carbide powder, and cobalt is coated on the surface of the tungsten carbide powder.

[0086] Depend on Figure 2 It can be seen that the tungsten carbide-cobalt reinforced copper-based composite coating prepared in Example 1 has a dense structure, and the tungsten carbide-cobalt composite powder is evenly dispersed in the copper base layer.

[0087] Depend on Figure 3 It can be seen that in the tungsten carbide-cobalt reinforced copper-based composite coating prepared in Example 1, cobalt is still well coated on the surface of the tungsten carbide powder, which greatly enhances the bonding force of the tungsten carbide powder in the composite coating.

[0088] Test Example 2

[0089] The coatings prepared in Examples 1-2 and Comparative Examples 1-2 were subjected to a reciprocating friction and wear test. The test conditions were: using a silicon nitride grinding ball with a diameter of 6.35 mm, applying a normal load of 20 N, a scratch distance of 5 mm, a sliding frequency of 2 Hz, and a test time of 20 min. The friction coefficient and wear rate of the coatings were measured. The results are shown in Table 1 and Figures 4 to 9 shown.

[0090]

[0091] Depend on Figures 4 to 9 It can be seen that, compared with the coatings prepared in Comparative Examples 1 to 2, under the same test conditions, the wear scar of the tungsten carbide-cobalt reinforced copper-based composite coating provided by the present invention is narrower, and the friction coefficient shows a significant downward trend with the increase of friction time. This indicates that the tungsten carbide-cobalt reinforced copper-based composite coating prepared by the present invention has a lower wear rate and a smaller friction coefficient than the copper coating and the tungsten carbide reinforced copper-based composite coating, and has better friction and wear resistance.

[0092] It can be seen from Table 1 that the tungsten carbide-cobalt reinforced copper-based composite coating prepared by the preparation method provided by the present invention has a smaller friction coefficient and a smaller wear rate than the copper coating and the tungsten carbide reinforced copper-based composite coating, and has better friction and wear resistance.

[0093] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A tungsten carbide-cobalt reinforced copper-based composite coating, comprising a tungsten carbide-cobalt composite powder and copper powder; the tungsten carbide-cobalt composite powder comprises a tungsten carbide powder and a cobalt metal layer coated on the surface of the tungsten carbide powder; the mass ratio of the tungsten carbide-cobalt composite powder to the copper powder is 1:9 to 2:3; the mass fraction of cobalt in the tungsten carbide-cobalt composite powder is 5 to 15%.

2. The method for preparing the tungsten carbide-cobalt reinforced copper-based composite coating according to claim 1, comprising the following steps: Mixing tungsten carbide powder with chemical activation liquid and performing activation treatment to obtain activated tungsten carbide powder; The activated tungsten carbide powder is mixed with a cobalt-containing chemical plating solution, and a cobalt metal layer is formed on the surface of the activated tungsten carbide powder through chemical plating to obtain a tungsten carbide-cobalt composite powder; The tungsten carbide-cobalt composite powder and copper powder are mixed to obtain a tungsten carbide-cobalt reinforced copper-based composite coating.

3. The preparation method according to claim 2, characterized in that: The chemical activation solution comprises hydrofluoric acid, nitric acid, ammonium fluoride and water; the content of hydrofluoric acid in the chemical activation solution is 20-40 mL / L, the content of nitric acid is 30-60 mL / L, and the content of ammonium fluoride is 2-5 g / L; the concentration of the hydrofluoric acid is 40 wt %, and the concentration of the nitric acid is 98 wt %.

4. The preparation method according to claim 2, characterized in that: The cobalt-containing chemical plating solution comprises cobalt sulfate, sodium hypophosphite, trisodium citrate, boric acid and water; the content of cobalt sulfate in the cobalt-containing chemical plating solution is 20-30 g / L, the content of sodium hypophosphite is 20-30 g / L, the content of trisodium citrate is 40-60 g / L, and the content of boric acid is 20-30 g / L; the pH value of the cobalt-containing chemical plating solution is 9-11.

5. The preparation method according to claim 2, characterized in that: The average particle size of the tungsten carbide powder is 5 to 30 μm; the average particle size of the tungsten carbide-cobalt composite powder is 5 to 32 μm; and the average particle size of the copper powder is 10 to 40 μm.

6. A method for preparing a tungsten carbide-cobalt reinforced copper-based composite coating, comprising the following steps: A tungsten carbide-cobalt reinforced copper-based composite coating is sprayed onto the surface of a metal substrate by a cold spraying method, and a tungsten carbide-cobalt reinforced copper-based composite coating is obtained on the surface of the metal substrate; the tungsten carbide-cobalt reinforced copper-based composite coating is the tungsten carbide-cobalt reinforced copper-based composite coating according to claim 1 or the tungsten carbide-cobalt reinforced copper-based composite coating prepared by the preparation method according to any one of claims 2 to 5.

7. The preparation method according to claim 6, characterized in that: The operating conditions of the cold spraying method include: the carrier gas is nitrogen; the spraying temperature is 500-700° C.; the spraying pressure is 2.5-5 MPa; and the spraying distance is 20-40 mm.

8. The tungsten carbide-cobalt reinforced copper-based composite coating prepared by the preparation method according to claim 6 or 7, comprising a copper-based layer, tungsten carbide particles doped in the copper-based layer, and a cobalt metal layer located between the copper-based layer and the tungsten carbide.