A preparation method of a universal lithium magnesium silicate paint mist coagulant

The universal lithium magnesium silicate paint mist coagulant method addresses the limitations of separate Agent A and B by forming larger paint mist agglomerates and enhancing water purification, simplifying operation and broadening applicability.

CN115849529BActive Publication Date: 2024-12-03FUJIAN TIANZE ENVIRONMENTAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211474611.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-23
Publication Date
2024-12-03
Estimated Expiration
2042-11-23

AI Technical Summary

Technical Problem

Existing paint mist coagulants require separate use of Agent A and Agent B, limiting their application scenarios and complicating the operation process, and are not universally applicable across different environments.

Method used

A method for preparing a universal lithium magnesium silicate paint mist coagulant using specific ratios of lithium magnesium silicate, sodium hydroxide, disinfectant, treatment agent, and additives, including polyepichlorohydrin-dimethylamine, polyaluminium chloride, polyacrylamide, and activated carbon, to neutralize paint mist charge, form larger agglomerates, and facilitate removal.

Benefits of technology

The method effectively condenses paint mist into larger agglomerates for easy removal, enhances water purification by removing heavy metals, and improves operational efficiency by simplifying the application process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115849529B_ABST
    Figure CN115849529B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of paint mist coagulants, and specifically, to a method for preparing a universal lithium magnesium silicate paint mist coagulant. The method comprises the following steps: weighing raw materials; putting lithium magnesium silicate into a reactor and adding deionized water to fully dissolve it, adding sodium hydroxide into the reactor and mixing it to produce a base liquid; injecting deionized water into a stirring barrel and preheating it, and sequentially putting a treatment agent and an additive into the stirring barrel and stirring it to produce a treatment liquid; after the base liquid and the treatment liquid are fully mixed, a disinfectant is put into the mixed liquid and stirred to produce a mother liquid and then allowed to stand; after removing the precipitate in the mother liquid, the mother liquid is subjected to low-temperature dehydration under vacuum conditions to produce a powdered paint mist coagulant. The present invention can remove the viscosity of the paint mist by adding a treatment agent and an additive, so that the paint mist condenses in water to form larger agglomerates, and has a good water purification effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of paint mist coagulants, in particular to a method for preparing a universal lithium magnesium silicate paint mist coagulant. Background Art

[0002] During the air painting process, a large amount of paint mist and organic solvent gas are generated, which will adhere to the inside of the equipment, pipes, fans and pumps, causing blockage of water and gas paths, seriously polluting the surrounding air and environment, and affecting the health of the operator. In order to extend the service life of the equipment and improve the working environment, paint mist coagulants are used to remove the sticky slag from the paint mist, thereby treating the paint mist.

[0003] Paint mist coagulant is a chemical agent specially used to remove paint from circulating water in water curtain spray rooms. Paint mist coagulant is an essential additive for spray treatment of circulating water in the paint spraying industry. Its main functions are: eliminating the viscosity of paint mist, condensing the paint mist into flocs and making it float on the surface of circulating water, so that it is easy to salvage and remove.

[0004] However, the existing paint mist coagulants are divided into Agent A for removing the stickiness of paint dropped in the water and Agent B for agglomerating and suspending the paint residue in the water. Agent A is generally injected at the circulating water pump port, and Agent B is generally injected at the return water port of the circulating water pool, that is, the two agents need to be separated and used in different places. The operation process is relatively cumbersome and the application scenarios are limited. It cannot be applied to paint mist treatment in different environments. Therefore, a preparation method of a universal lithium magnesium silicate paint mist coagulant is proposed. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing a universal lithium magnesium silicate paint mist coagulant to solve the problems raised in the above background technology.

[0006] To achieve the above object, the present invention provides a method for preparing a universal lithium magnesium silicate paint mist coagulant, comprising the following steps:

[0007] S1. Weigh 54-78 parts by weight of lithium magnesium silicate, 10-21 parts by weight of sodium hydroxide, 8-16 parts by weight of a disinfectant, 3-9 parts by weight of a treatment agent, and 3-7 parts by weight of an additive;

[0008] S2, putting lithium magnesium silicate into a reactor and adding deionized water to fully dissolve it, then adding sodium hydroxide into the reactor and mixing to produce a base solution;

[0009] S3, injecting deionized water into the stirring barrel and preheating it, and sequentially adding a treatment agent and an additive into the stirring barrel and stirring to produce a treatment liquid;

[0010] S4, after the base liquid and the treatment liquid are fully mixed, a disinfectant is added to the mixed liquid and stirred evenly to produce a mother liquid and then allowed to stand;

[0011] S5. After removing the precipitate from the mother liquor, the mother liquor is dehydrated at low temperature under vacuum conditions to prepare a powdered paint mist coagulant.

[0012] As a further improvement of the present technical solution, the disinfectant is a di-long-chain quaternary ammonium salt disinfectant.

[0013] As a further improvement of the technical solution, the treating agent includes polyepichlorohydrin-dimethylamine and polyaluminium chloride.

[0014] As a further improvement of the technical solution, the additives include polyacrylamide and activated carbon.

[0015] As a further improvement of the present technical solution, in S2, the solution is mixed by a vortex mixer.

[0016] As a further improvement of the technical solution, in S3, the preheating temperature is 25-40°C.

[0017] As a further improvement of the technical solution, in S3, the mass fraction of the solute in the treatment liquid is 10-25%.

[0018] As a further improvement of the technical solution, in S4, the stirring speed is 25-55 rpm / min.

[0019] As a further improvement of the present technical solution, in S5, the powder particle size of the paint mist coagulant is 28-41 μm.

[0020] In the present invention, a treatment agent is added to neutralize the negative charge of the paint mist in the water to remove the viscosity of the paint mist, so that the paint mist forms unstable fine particles in the water and then condenses to form larger agglomerates, thereby facilitating the removal of paint mist residues. Polyepichlorohydrin-dimethylamine is a polymer surfactant that can combine with the negatively charged groups of the paint mist in the water to eliminate the negative charge of the paint mist to reduce or remove the viscosity of the paint mist residues. Polyaluminium chloride is a polymer coagulant that adsorbs and bridges the polymer substance with the colloid particles in the water. During the hydrolysis process, physical and chemical processes such as condensation, adsorption and precipitation occur, thereby achieving condensation and sedimentation of the paint mist in the water. By adding additives, the paint mist in the water can be removed. Heavy metals have good water purification effects. Polyacrylamide can reduce water resistance to facilitate the flow of condensed paint mist residues. Activated carbon has good adsorption properties and can effectively remove harmful substances in water. Among them, after polyacrylamide is dissolved in water, the number of cationic groups in the molecular chain is larger than that of anionic groups, and the positive charge is larger. The cations produced by the hydrolysis of polyepichlorohydrin-dimethane can effectively neutralize the negative charge of paint mist. In addition, polyacrylamide presents a network structure after being dissolved in water, and the mechanical entanglement and hydrogen bonds between its chains form network nodes together, which improves the cohesion strength of the paint mist residues and accelerates the purification speed of the water body, thereby realizing the treatment of the paint mist residues.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] In the preparation method of the universal lithium magnesium silicate paint mist coagulant, the viscosity of the paint mist can be removed by adding a treatment agent, so that the paint mist can be condensed in water to form larger agglomerates, and heavy metals in the water can be removed by adding additives, thereby having a good water purification effect. Among them, after polyacrylamide is dissolved in water, the number of cationic groups in the molecular chain is relatively large relative to the number of anionic groups, and the combination with polyepichlorohydrin-dimethane can effectively neutralize the negative charge of the paint mist. In addition, after polyacrylamide is dissolved in water, it presents a network structure, and the mechanical entanglement and hydrogen bonds between the chains jointly form network nodes, thereby improving the cohesion strength of the paint mist residue and accelerating the purification speed of the water body, thereby realizing the treatment of the paint mist residue. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is the overall flow chart of the present invention. DETAILED DESCRIPTION

[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] See also Figure 1 As shown, the object of the present invention is to provide a method for preparing a universal lithium magnesium silicate paint mist coagulant, comprising the following steps:

[0026] S1, weighing 54-78 parts by weight of lithium magnesium silicate, 10-21 parts by weight of sodium hydroxide, 8-16 parts by weight of disinfectant, 3-9 parts by weight of treatment agent and 3-7 parts by weight of additives, wherein the disinfectant is a di-long chain quaternary ammonium salt disinfectant, which is a high-level disinfectant with mild performance. By adding a quaternary ammonium salt disinfectant, most bacterial propagules in water can be killed to prevent water deterioration caused by bacterial growth. The treatment agent includes polyepichlorohydrin-dimethylamine and polyaluminum chloride. By adding the treatment agent, the negative charge of the paint mist in the water can be neutralized to remove the viscosity of the paint mist, so that the paint mist forms unstable fine particles in the water and then condenses to form larger agglomerates, thereby facilitating the removal of paint mist residues. The additive includes polyacrylamide and activated carbon. By adding the additive, heavy metals in the water can be removed, and a good water purification effect is achieved.

[0027] S2, putting lithium magnesium silicate into a reactor and adding deionized water to fully dissolve it, adding sodium hydroxide into the reactor and mixing the solution with a vortex mixer to produce a base solution, wherein the vortex mixer uses eccentric rotation to generate a vortex in the liquid in a container such as a test tube, so that the solution is fully mixed;

[0028] S3, injecting deionized water into the stirring barrel and preheating it, and sequentially adding the treatment agent and the additive into the stirring barrel and stirring to produce the treatment liquid, wherein the preheating temperature is 25-40°C, and the deionized water is heated to increase the temperature, which is conducive to the dissolution of the treatment agent and the additive in the deionized water, and the mass fraction of the solute in the treatment liquid is 10-25%. When the concentration of the treatment liquid is high, the polymer groups dissolved in the water will penetrate each other, making the treatment liquid a gel with high viscosity, which is not conducive to the mixing of the materials, so the mass fraction value of the solute in the treatment liquid is set to be low;

[0029] S4. After the base liquid and the treatment liquid are fully mixed, a disinfectant is added to the mixed liquid and stirred at a speed of 25-55 rpm / min to produce a mother liquid, and then allowed to stand, and the disinfectant is fully dissolved in the mixed liquid by stirring to ensure that the components in the mixed liquid are evenly mixed;

[0030] S5. After removing the precipitate from the mother liquor, the mother liquor is subjected to low-temperature dehydration under vacuum conditions to prepare a powdered paint mist coagulant with a powder particle size of 28-41 μm. The smaller the powder particle size, the faster the dissolution rate of the paint mist coagulant during use, which is beneficial to the treatment of paint mist residues.

[0031] In the present invention, a treatment agent is added to neutralize the negative charge of the paint mist in the water to remove the viscosity of the paint mist, so that the paint mist forms unstable fine particles in the water and then condenses to form larger agglomerates, thereby facilitating the removal of paint mist residues. Polyepichlorohydrin-dimethylamine is a polymer surfactant that can combine with the negatively charged groups of the paint mist in the water to eliminate the negative charge of the paint mist to reduce or remove the viscosity of the paint mist residues. Polyaluminium chloride is a polymer coagulant that adsorbs and bridges the polymer substance with the colloid particles in the water. During the hydrolysis process, physical and chemical processes such as condensation, adsorption and precipitation occur, thereby achieving condensation and sedimentation of the paint mist in the water. By adding additives, the paint mist in the water can be removed. Heavy metals have good water purification effects. Polyacrylamide can reduce water resistance to facilitate the flow of condensed paint mist residues. Activated carbon has good adsorption properties and can effectively remove harmful substances in water. Among them, after polyacrylamide is dissolved in water, the number of cationic groups in the molecular chain is larger than that of anionic groups, and the positive charge is larger. The cations produced by the hydrolysis of polyepichlorohydrin-dimethane can effectively neutralize the negative charge of paint mist. In addition, polyacrylamide presents a network structure after being dissolved in water, and the mechanical entanglement and hydrogen bonds between its chains form network nodes together, which improves the cohesion strength of the paint mist residues and accelerates the purification speed of the water body, thereby realizing the treatment of the paint mist residues.

[0032] According to the differences in the amount of raw materials and process parameters during the preparation process, the general-purpose lithium magnesium silicate paint mist coagulant prepared by the present invention is further described through the following specific examples.

[0033] Example 1

[0034] S1, weighing 54 parts by weight of lithium magnesium silicate, 10 parts by weight of sodium hydroxide, 8 parts by weight of a disinfectant, 3 parts by weight of a treating agent and 3 parts by weight of an additive, wherein the disinfectant is a di-long-chain quaternary ammonium salt disinfectant, the treating agent includes polyepichlorohydrin-dimethylamine and polyaluminium chloride, and the additive includes polyacrylamide and activated carbon;

[0035] S2, putting lithium magnesium silicate into a reactor and adding deionized water to fully dissolve it, then adding sodium hydroxide into the reactor and mixing the solution with a vortex mixer to produce a base solution;

[0036] S3, injecting deionized water into the stirring barrel and preheating it, and sequentially adding a treatment agent and an additive into the stirring barrel and stirring to produce a treatment liquid, wherein the preheating temperature is 25° C., and the mass fraction of the solute in the treatment liquid is 10%;

[0037] S4. After the base liquid and the treatment liquid are fully mixed, a disinfectant is added to the mixed liquid and stirred at a speed of 25 rpm / min to produce a mother liquid and then allowed to stand;

[0038] S5. After removing the precipitate from the mother liquor, the mother liquor is subjected to low-temperature dehydration under vacuum conditions to prepare a powdered paint mist coagulant with a powder particle size of 28 μm.

[0039] Example 2

[0040] S1, weighing 63 parts by weight of lithium magnesium silicate, 15 parts by weight of sodium hydroxide, 12 parts by weight of a disinfectant, 5 parts by weight of a treating agent and 4 parts by weight of an additive, wherein the disinfectant is a di-long-chain quaternary ammonium salt disinfectant, the treating agent includes polyepichlorohydrin-dimethylamine and polyaluminium chloride, and the additive includes polyacrylamide and activated carbon;

[0041] S2, putting lithium magnesium silicate into a reactor and adding deionized water to fully dissolve it, then adding sodium hydroxide into the reactor and mixing the solution with a vortex mixer to produce a base solution;

[0042] S3, injecting deionized water into the stirring barrel and preheating it, and sequentially adding a treatment agent and an additive into the stirring barrel and stirring to produce a treatment liquid, wherein the preheating temperature is 33° C., and the mass fraction of the solute in the treatment liquid is 18%;

[0043] S4. After the base liquid and the treatment liquid are fully mixed, a disinfectant is added to the mixed liquid and stirred at a speed of 40 rpm / min to produce a mother liquid and then allowed to stand;

[0044] S5. After removing the precipitate from the mother liquor, the mother liquor is subjected to low-temperature dehydration under vacuum conditions to prepare a powdered paint mist coagulant with a powder particle size of 35 μm.

[0045] Example 3

[0046] S1, weighing 78 parts by weight of lithium magnesium silicate, 21 parts by weight of sodium hydroxide, 16 parts by weight of a disinfectant, 9 parts by weight of a treating agent and 7 parts by weight of an additive, wherein the disinfectant is a di-long-chain quaternary ammonium salt disinfectant, the treating agent includes polyepichlorohydrin-dimethylamine and polyaluminium chloride, and the additive includes polyacrylamide and activated carbon;

[0047] S2, putting lithium magnesium silicate into a reactor and adding deionized water to fully dissolve it, then adding sodium hydroxide into the reactor and mixing the solution with a vortex mixer to produce a base solution;

[0048] S3, injecting deionized water into the stirring barrel and preheating it, and sequentially adding a treatment agent and an additive into the stirring barrel and stirring to produce a treatment liquid, wherein the preheating temperature is 40° C., and the mass fraction of the solute in the treatment liquid is 25%;

[0049] S4. After the base liquid and the treatment liquid are fully mixed, a disinfectant is added to the mixed liquid and stirred at a speed of 55 rpm / min to produce a mother liquid and then allowed to stand;

[0050] S5. After removing the precipitate from the mother liquor, the mother liquor is subjected to low-temperature dehydration under vacuum conditions to prepare a powdered paint mist coagulant with a powder particle size of 41 μm.

[0051] Example 4

[0052] S1, weighing 55 parts by weight of lithium magnesium silicate, 20 parts by weight of sodium hydroxide, 10 parts by weight of a disinfectant, 8 parts by weight of a treating agent and 5 parts by weight of an additive, wherein the disinfectant is a di-long-chain quaternary ammonium salt disinfectant, the treating agent includes polyepichlorohydrin-dimethylamine and polyaluminium chloride, and the additive includes polyacrylamide and activated carbon;

[0053] S2, putting lithium magnesium silicate into a reactor and adding deionized water to fully dissolve it, then adding sodium hydroxide into the reactor and mixing the solution with a vortex mixer to produce a base solution;

[0054] S3, injecting deionized water into the stirring barrel and preheating it, and sequentially adding a treatment agent and an additive into the stirring barrel and stirring to produce a treatment liquid, wherein the preheating temperature is 25° C., and the mass fraction of the solute in the treatment liquid is 20%;

[0055] S4. After the base liquid and the treatment liquid are fully mixed, a disinfectant is added to the mixed liquid and stirred at a speed of 50 rpm / min to produce a mother liquid and then allowed to stand;

[0056] S5. After removing the precipitate from the mother liquor, the mother liquor is subjected to low-temperature dehydration under vacuum conditions to prepare a powdered paint mist coagulant with a powder particle size of 30 μm.

[0057] Table 1 Comparison of the amount of each raw material in Examples 1-4

[0058] Example 1 Example 2 Example 3 Example 4 Lithium magnesium silicate / part 54 63 78 55 Sodium hydroxide / part 10 15 21 20 Disinfectant / unit 8 12 16 10 Treatment agent / unit 3 5 9 8 Additives / portion 3 4 7 5

[0059] Table 2 Comparison of process parameters in Examples 1-4

[0060]

[0061] Comparative Example 1

[0062] This comparative example adopts the preparation process of Example 1, only lacking the treatment agent, and the rest remains unchanged, and the specific steps are as follows:

[0063] S1. Weigh 54 parts by weight of lithium magnesium silicate, 10 parts by weight of sodium hydroxide, 8 parts by weight of a disinfectant, and 3 parts by weight of an additive, wherein the disinfectant is a di-long-chain quaternary ammonium salt disinfectant, and the additive includes polyacrylamide and activated carbon;

[0064] S2, putting lithium magnesium silicate into a reactor and adding deionized water to fully dissolve it, then adding sodium hydroxide into the reactor and mixing the solution with a vortex mixer to produce a base solution;

[0065] S3, injecting deionized water into the stirring barrel and preheating it, adding additives into the stirring barrel and stirring to produce a treatment liquid, wherein the preheating temperature is 25° C., and the mass fraction of the solute in the treatment liquid is 10%;

[0066] S4. After the base liquid and the treatment liquid are fully mixed, a disinfectant is added to the mixed liquid and stirred at a speed of 25 rpm / min to produce a mother liquid and then allowed to stand;

[0067] S5. After removing the precipitate from the mother liquor, the mother liquor is subjected to low-temperature dehydration under vacuum conditions to prepare a powdered paint mist coagulant with a powder particle size of 28 μm.

[0068] Comparative Example 2

[0069] This comparative example adopts the preparation process of Example 2, except that the treatment agent is missing and the rest remains unchanged. The specific steps are similar to those of Comparative Example 1, and will not be repeated in this comparative example.

[0070] Comparative Example 3

[0071] This comparative example adopts the preparation process of Example 3, except that the treatment agent is missing and the rest remains unchanged. The specific steps are similar to those of Comparative Example 1, and will not be repeated in this comparative example.

[0072] Comparative Example 4

[0073] This comparative example adopts the preparation process of Example 4, only lacking the treatment agent, and the rest remains unchanged. The specific steps are similar to those of Comparative Example 1, and this comparative example will not be repeated.

[0074] Table 3 Comparison of the amount of each raw material in Comparative Examples 1-4

[0075] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Lithium magnesium silicate / part 54 63 78 55 Sodium hydroxide / part 10 15 21 20 Disinfectant / unit 8 12 16 10 Treatment agent / unit / / / / Additives / portion 3 4 7 5

[0076] Comparative Example 5

[0077] This comparative example adopts the preparation process of Example 1, only lacking the additives, and the rest remains unchanged, and the specific steps are as follows:

[0078] S1, weighing 54 parts by weight of lithium magnesium silicate, 10 parts by weight of sodium hydroxide, 8 parts by weight of a disinfectant and 3 parts by weight of a treating agent, wherein the disinfectant is a di-long-chain quaternary ammonium salt disinfectant, and the treating agent includes polyepichlorohydrin-dimethylamine and polyaluminium chloride;

[0079] S2, putting lithium magnesium silicate into a reactor and adding deionized water to fully dissolve it, then adding sodium hydroxide into the reactor and mixing the solution with a vortex mixer to produce a base solution;

[0080] S3, injecting deionized water into the stirring barrel and preheating it, adding a treatment agent into the stirring barrel and stirring to produce a treatment liquid, wherein the preheating temperature is 25° C., and the mass fraction of the solute in the treatment liquid is 10%;

[0081] S4. After the base liquid and the treatment liquid are fully mixed, a disinfectant is added to the mixed liquid and stirred at a speed of 25 rpm / min to produce a mother liquid and then allowed to stand;

[0082] S5. After removing the precipitate from the mother liquor, the mother liquor is subjected to low-temperature dehydration under vacuum conditions to prepare a powdered paint mist coagulant with a powder particle size of 28 μm.

[0083] Comparative Example 6

[0084] This comparative example adopts the preparation process of Example 4, only the additive is missing, and the rest remains unchanged. The specific steps are similar to those of Comparative Example 5, and this comparative example will not be repeated.

[0085] Comparative Example 7

[0086] This comparative example adopts the preparation process of Example 5, only lacking the additives, and the rest remains unchanged. The specific steps are similar to those of Comparative Example 5, and this comparative example will not be repeated.

[0087] Comparative Example 8

[0088] This comparative example adopts the preparation process of Example 5, only lacking the additives, and the rest remains unchanged. The specific steps are similar to those of Comparative Example 5, and this comparative example will not be repeated.

[0089] Table 4 Comparison of the amount of each raw material in comparative examples 5-8

[0090] Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 Lithium magnesium silicate / part 54 63 78 55 Sodium hydroxide / part 10 15 21 20 Disinfectant / unit 8 12 16 10 Treatment agent / unit 3 5 9 8 Additives / portion / / / /

[0091] Table 5 Comparison of process parameters in comparative examples 1-8

[0092]

[0093] Comparative Example 9

[0094] This comparative example is based on comparative example 1, except that the preheating temperature is set to 50° C., and the rest remain unchanged. The specific steps are similar to those in comparative example 1, and will not be described in detail in this comparative example.

[0095] Comparative Example 10

[0096] This comparative example is based on comparative example 2, except that the mass fraction of the solute is set to 30%, and the rest remain unchanged. The specific steps are similar to those in comparative example 2, and will not be described in detail in this comparative example.

[0097] Comparative Example 11

[0098] This comparative example is based on comparative example 3, except that the stirring speed is set to 20 rpm / min, and the rest remain unchanged. The specific steps are similar to those of comparative example 3, and will not be repeated in this comparative example.

[0099] Comparative Example 12

[0100] In this comparative example, on the basis of comparative example 4, the powder particle size is set to 45 μm, and the rest remains unchanged. The specific steps are similar to those in comparative example 4, and will not be described in detail in this comparative example.

[0101] Table 6 Comparison of the amount of each raw material in comparative examples 9-12

[0102]

[0103]

[0104] Table 7 Comparison of process parameters in comparative examples 9-12

[0105]

[0106] Test example

[0107] The paint mist coagulants prepared in Examples 1-4 and Comparative Examples 1-12 were tested for their coagulation and floating effects. Paint was placed in a water pool, and at room temperature of 30°C and humidity of 50% RH, the paint mist coagulants prepared in the examples and comparative examples were respectively put into the water pool. After 3 minutes, the floating degree of the paint in the water pool, that is, the proportion of the floated paint in the total amount of paint, was observed, and the generated paint mist residue was scored. The scoring criteria are shown in Table 8, and the average score of each paint mist coagulant and the degree of paint floating are filled in Table 9.

[0108] Table 8 Scoring criteria

[0109]

[0110]

[0111] Table 9 Test comparison of paint mist coagulants prepared by the embodiments and comparative examples

[0112] Paint floating degree / % Average score Example 1 98.7 4.63 Example 2 99.1 4.73 Example 3 99.0 4.71 Example 4 98.9 4.67 Comparative Example 1 95.8 4.41 Comparative Example 2 96.2 4.50 Comparative Example 3 96.0 4.46 Comparative Example 4 95.8 4.42 Comparative Example 5 95.7 4.39 Comparative Example 6 96.1 4.48 Comparative Example 7 96.0 4.45 Comparative Example 8 95.9 4.44 Comparative Example 9 95.5 4.36 Comparative Example 10 96.0 4.46 Comparative Example 11 95.7 4.40 Comparative Example 12 95.5 4.35

[0113] According to Table 9, when comparing the paint mist coagulants prepared using Examples 1-4 with the paint mist coagulants prepared using Comparative Examples 1-12, the paint floating degree and the average score of the paint mist coagulants of the examples are greater than the paint floating degree and the average score of the paint mist coagulants of the comparative examples, and the paint floating degree of the paint mist coagulants of the examples is higher than 98.7%, and the average score is higher than 4.63, while the paint floating degree and the average score of the paint mist coagulants prepared using the comparative examples with different raw material amounts and process parameters are decreased. Therefore, the paint mist coagulants prepared by the present invention have a good paint residue coagulation and floating effect.

[0114] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a universal lithium magnesium silicate paint mist coagulant, It is characterized in that The following steps are involved: S1. Weigh 54-78 parts by weight of lithium magnesium silicate, 10-21 parts by weight of sodium hydroxide, 8-16 parts by weight of a disinfectant, 3-9 parts by weight of a treatment agent, and 3-7 parts by weight of an additive; S2, putting lithium magnesium silicate into a reactor and adding deionized water to fully dissolve it, then adding sodium hydroxide into the reactor and mixing to produce a base solution; S3, injecting deionized water into the stirring barrel and preheating it, and sequentially adding a treatment agent and an additive into the stirring barrel and stirring to produce a treatment liquid; S4, after the base liquid and the treatment liquid are fully mixed, a disinfectant is added to the mixed liquid and stirred evenly to produce a mother liquid and then allowed to stand; S5, after removing the precipitate in the mother liquor, dehydrating the mother liquor at low temperature under vacuum conditions to prepare a powdered paint mist coagulant; The disinfectant is a di-long-chain quaternary ammonium salt disinfectant; The treating agent includes polyepichlorohydrin-dimethylamine and polyaluminium chloride; The additives include polyacrylamide and activated carbon.

2. A method for preparing a universal lithium magnesium silicate paint mist coagulant according to claim 1, Features: In S2, the solution is mixed by a vortex mixer.

3. A method for preparing a universal lithium magnesium silicate paint mist coagulant according to claim 1, Features: In S3, the preheating temperature is 25-40°C.

4. A method for preparing a universal lithium magnesium silicate paint mist coagulant according to claim 1, Features: In S3, the mass fraction of the solute in the treatment liquid is 10-25%.

5. A method for preparing a universal lithium magnesium silicate paint mist coagulant according to claim 1, Features: In S4, the stirring speed is 25-55 rpm / min.

6. A method for preparing a universal lithium magnesium silicate paint mist coagulant according to claim 1, Features: In the S5, the powder particle size of the paint mist coagulant is 28-41 μm.