A kind of anti-mildew glue for building construction and preparation method thereof

Through the combination of alkoxy silicon-based modified polymer and synergistic additives, the problem of mildew-proof glue degradation and incomplete filling under running water erosion is solved, the mechanical properties and mildew-proof effect of mildew-proof glue are improved, and the Anti-mold time and improve safety and environmental protection.

CN115851204BActive Publication Date: 2024-11-15ANHUI NIUYUAN NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210303424.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-24
Publication Date
2024-11-15
Estimated Expiration
2042-03-24

AI Technical Summary

Technical Problem

The existing anti-mold glue gradually disappears under running water erosion, and there may be problems of incomplete filling at the joints of the tile, which affects the performance and is poor in safety and environmental protection.

Method used

Using a combination of alkoxysilyl modified polymers, plasticizers, fillers and additives, diethylene triamine propyl trimethoxysilane and isopropyl tris(dioctylphosphate acyloxy)titanic acid The synergistic effect of the ester coupling agent and inorganic silver ions and zinc oxide improves the mechanical properties and anti-mold effect of anti-mold glue, prevents the precipitation of anti-mold agents and prolongs the anti-mold time.

Benefits of technology

It improves the elastic recovery rate and fracture elongation rate of anti-mold glue, prevents the joints from being filled with imperfectly, prolongs the durability of the anti-mold effect, and improves safety and environmental protection.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A kind of external mildew-proof glue for construction, the raw materials for preparing the materials include by weight: 30-60 parts of alkoxysilyl modified polymer, 10-20 parts of plasticizer, 20-30 parts of filler, 5-10 parts of auxiliary agent, and 1-5 parts of color paste. The present invention adopts the synergistic effect of dimethoxysilyl-terminated polyether with a viscosity of 5-50Pa.s and polypropylene with a molecular weight of 2000-4000 Dalton, so that the mildew-proof glue has good elastic recovery rate and elongation at break, effectively preventing the problem of incomplete joint filling caused by shrinkage after tile bonding and curing; and by adopting a combination of diethylenetriamine propyl trimethoxysilane and isopropyl tri (dioctyl phosphate acyloxy) titanate, the binding of inorganic filler and mildew-proof agent to polymer is increased, and the mildew-proof effect caused by the precipitation of mildew-proof agent is effectively prevented from decreasing. At the same time, inorganic silver ions and zinc oxide are used in coordination as mildew-proof agent, so that mildew-proof agent can have a sustained release effect and extend the mildew-proof time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an anti-mildew glue for external use in building construction, relates to C09J, and specifically relates to the field of adhesives. Background Art

[0002] As people's living standards improve, they pay more and more attention to their physical health. Bacteria are particularly prone to breeding in humid indoor environments, which can easily cause diseases after contact. Therefore, people will lay tiles in dark and humid places such as bathrooms, kitchens, and basements to prevent moisture from accumulating on the floor and walls and causing bacteria to grow. However, the joints of the tiles will inevitably come into contact with moisture, causing the growth of bacteria. Therefore, it is necessary to use anti-mildew glue to seal the joints of the tiles. However, the anti-mildew properties of the anti-mildew glue on the market will gradually disappear under the erosion of running water, and the anti-mildew effect is not long-lasting.

[0003] Chinese invention patent CN201910054716.2 discloses a real porcelain kitchen and bathroom mildew-proof glue and its preparation method. The material uses a silicone-modified polyether resin with a high cross-linking density, so that the colloid can maintain a very high hardness. However, when sealing the joints of tiles, the tiles will shrink after being bonded and cured to the wall. The high-hardness mildew-proof glue may not fill the joints completely, affecting the performance. Chinese invention patent CN201811600114.4 discloses a silane-modified mildew-proof glue and its preparation method. The sealing effect is achieved by curing and cross-linking under water vapor conditions, and the performance is stable under normal temperature conditions. However, tin catalysts and benzene plasticizers are used, and the safety and environmental protection are poor. Summary of the invention

[0004] In order to improve the mechanical properties of anti-mildew glue and extend the anti-mildew time, the first aspect of the present invention provides an anti-mildew glue for external use in construction. The preparation raw materials include, by weight: 30-60 parts of alkoxysilane-modified polymer, 10-20 parts of plasticizer, 20-30 parts of filler, 5-10 parts of auxiliary agent, and 1-5 parts of color paste.

[0005] As a preferred embodiment, the raw materials for preparation include, by weight: 40-55 parts of alkoxysilyl modified polymer, 13-18 parts of plasticizer, 23-26 parts of filler, 6-8 parts of auxiliary agent, and 2-4 parts of color paste.

[0006] As a preferred embodiment, the raw materials for preparation include, by weight: 50 parts of alkoxysilyl modified polymer, 15 parts of plasticizer, 25 parts of filler, 7 parts of auxiliary agent, and 3 parts of color paste.

[0007] As a preferred embodiment, the alkoxysilyl modified polymer is selected from one or a combination of dimethoxysilyl terminated polyether, trimethoxysilane terminated polyether, and silyl polyether acrylate.

[0008] As a preferred embodiment, the alkoxysilyl modified polymer is a dimethoxysilyl terminated polyether.

[0009] As a preferred embodiment, the viscosity of the alkoxysilyl modified polymer at 25° C. is 5-50 Pa.s.

[0010] As a preferred embodiment, the viscosity of the alkoxysilyl modified polymer at 25° C. is 5-20 Pa.s.

[0011] As a preferred embodiment, the alkoxysilyl modified polymer has a viscosity of 13 Pa.s and 8 Pa.s at 25°C.

[0012] As a preferred embodiment, the weight ratio of the dimethoxysilyl-terminated polyether having a viscosity of 13 Pa.s and 8 Pa.s at 25° C. is 1:(0.2-0.5).

[0013] As a preferred embodiment, the weight ratio of the dimethoxysilyl-terminated polyethers having a viscosity of 13 Pa.s and 8 Pa.s at 25° C. is 1:0.3.

[0014] As a preferred embodiment, the plasticizer is selected from one or a combination of aliphatic dibasic acid esters, fatty acid esters, polyol esters, phosphate ester plasticizers, alkyl sulfonates, fatty alcohols, and polyester plasticizers.

[0015] As a preferred embodiment, the fatty alcohol is selected from one or a combination of n-hexanol, dodecanol, decanol, polyethylene glycol, polypropylene glycol, and palmityl alcohol. Preferably, the molecular weight of the polypropylene glycol is 2000-4000 Daltons.

[0016] As a preferred embodiment, the plasticizer is polypropylene glycol with a molecular weight of 3000-4000 Daltons. Preferably, the molecular weight of the polypropylene glycol is 3000 Daltons.

[0017] As a preferred embodiment, the filler is selected from one or a combination of light calcium carbonate, heavy calcium carbonate, and talcum powder, and the particle size of the light calcium carbonate is 0.1-1 μm.

[0018] As a preferred embodiment, the filler is a combination of light calcium carbonate and heavy calcium carbonate, the particle size of the light calcium carbonate is 0.1-0.5 μm, and the weight ratio of the light calcium carbonate to the heavy calcium carbonate is (1.5-2):1.

[0019] As a preferred embodiment, the weight ratio of the light calcium carbonate to the heavy calcium carbonate is 1.75:1.

[0020] As a preferred embodiment, the auxiliary agent is selected from one or a combination of mildew preventer, thixotropic agent, catalyst, coupling agent and light stabilizer. Preferably, the auxiliary agent is a combination of mildew preventer, thixotropic agent, catalyst and coupling agent; preferably, the weight ratio of mildew preventer, thixotropic agent, catalyst and coupling agent is (1-2): (1-2) (0.1-0.5): 1; more preferably, the weight ratio of mildew preventer, thixotropic agent, catalyst and coupling agent is 2:1:0.3:1.

[0021] As a preferred embodiment, the mildew preventer is selected from one or a combination of metal ion mildew preventers, metal oxide mildew preventers, quaternary ammonium salt mildew preventers, biguanide mildew preventers, and thiazole mildew preventers.

[0022] As a preferred embodiment, the mildew preventer is a combination of a metal ion mildew preventer and a metal oxide mildew preventer. Preferably, the mildew preventer is a combination of inorganic silver ions and zinc oxide.

[0023] As a preferred embodiment, the weight ratio of the inorganic silver ions to zinc oxide is 1:(1-2), and more preferably, the weight ratio of the inorganic silver ions to zinc oxide is 1:1.5.

[0024] As a preferred embodiment, the coupling agent is selected from one or a combination of aminosilane coupling agents, vinylsilane coupling agents, alkylsilane coupling agents, titanate coupling agents, and aluminate coupling agents.

[0025] As a preferred embodiment, the aminosilane coupling agent is diethylenetriaminopropyltrimethoxysilane, and the titanate coupling agent is isopropyl tri(dioctylphosphoyl) titanate; preferably, the coupling agent is a combination of diethylenetriaminopropyltrimethoxysilane and isopropyl tri(dioctylphosphoyl) titanate.

[0026] As a preferred embodiment, the weight ratio of diethylenetriaminopropyltrimethoxysilane to isopropyl tri(dioctylphosphoyl)titanate is 1:(0.5-1.5).

[0027] As a preferred embodiment, the weight ratio of diethylenetriaminopropyltrimethoxysilane to isopropyl tri(dioctylphosphoyl)titanate is 1:1.

[0028] The applicant found in the experiment that the combination of diethylenetriaminepropyl trimethoxysilane and isopropyl tri(dioctylphosphoyloxy) titanate can improve the binding performance of alkoxysilyl modified polymer with filler and mildew inhibitor. The non-polar group is combined with filler and mildew inhibitor, and the polar group is combined with polymer, which can increase the binding of inorganic filler and mildew inhibitor, avoid the precipitation of mildew inhibitor under the scouring of water flow, and lead to the decline of mildew inhibitor performance. In addition, the applicant found in the experiment that the synergistic effect of diethylenetriaminepropyl trimethoxysilane and isopropyl tri(dioctylphosphoyloxy) titanate can increase the tensile strength and elongation at break of alkoxysilyl modified polymer. It is speculated that the possible reason is that the polar group of the coupling agent can be interspersed between the chain segments of the polymer, promote the formation of a cross-linked network structure, and increase the mechanical properties and elastic recovery rate of the mildew-proof glue. At the same time, the applicant found that the synergistic effect of inorganic silver ions and zinc oxide can prolong the mildew-proof time of the mildew-proof glue. The possible reason is that zinc oxide can capture the photoelectron energy in the environment to generate hydroxyl free radicals and superoxide anions, which have a sustained and slow-release mildew-proof and bactericidal effect, thereby prolonging the mildew-proof effect time.

[0029] As a preferred embodiment, the catalyst is selected from one or a combination of organic tin catalysts, bismuth catalysts, organic zinc catalysts, and nitrogen heterocyclic olefin catalysts.

[0030] As a preferred embodiment, the catalyst is an organic zinc catalyst.

[0031] As a preferred embodiment, the thixotropic agent is selected from one or a combination of organic bentonite, fumed silica, and attapulgite.

[0032] As a preferred embodiment, the thixotropic agent is fumed silica.

[0033] The second aspect of the present invention provides a method for preparing an anti-mildew adhesive for building construction, comprising the following steps:

[0034] (1) Mix the alkoxysilane-modified polymer, plasticizer, mildew inhibitor, thixotropic agent and color paste in a vacuum mixture for 10-15 minutes;

[0035] (2) Then add coupling agent, light stabilizer and filler and continue stirring for 10-15 minutes;

[0036] (3) Finally, add the catalyst, stir for 5-10 minutes, discharge the material, and seal it.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] (1) The anti-mildew adhesive for external use in building construction of the present invention adopts a dimethoxysilyl-terminated polyether with a viscosity of 5-50 Pa.s and a polypropylene glycol with a molecular weight of 2000-4000 Daltons to cooperate with each other, so that the anti-mildew adhesive has good elastic recovery rate and elongation at break, and effectively prevents the problem of incomplete filling of joints caused by shrinkage of tiles after curing.

[0039] (2) The anti-mildew adhesive for external use in building construction of the present invention increases the binding property of inorganic filler, anti-mildew agent and polymer by adopting a combination of diethylenetriaminopropyltrimethoxysilane and isopropyl tri(dioctylphosphoyl)titanate, thereby effectively preventing the precipitation of anti-mildew agent and causing a decrease in anti-mildew effect.

[0040] (3) The anti-mildew adhesive for external use in building construction of the present invention increases the cross-linking density of the dimethoxysilyl-terminated polyether by adopting diethylenetriaminopropyltrimethoxysilane and isopropyl tri(dioctylphosphoyl)titanate in a weight ratio of 1:1, thereby improving the tensile strength and elongation at break of the anti-mildew adhesive.

[0041] (4) The anti-mildew adhesive for external use in building construction of the present invention adopts inorganic silver ions and zinc oxide as anti-mildew agents, which can make the anti-mildew agent have a certain slow-release effect and prolong the anti-mildew effect.

[0042] (5) The anti-mildew glue for external use in building construction of the present invention can improve the thixotropy of the anti-mildew colloid, reduce the sag, and improve the appearance of the colloid after curing by using light calcium carbonate and heavy calcium carbonate with a particle size of 0.1-1 μm. DETAILED DESCRIPTION

[0043] The present invention is described in detail below by way of examples. It is necessary to point out here that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by professionals and technicians in this field based on the content of the present invention above still belong to the scope of protection of the present invention.

[0044] In addition, unless otherwise stated, all raw materials used were commercially available.

[0045] Example 1

[0046] The invention discloses an anti-mildew adhesive for external use in building construction. The raw materials for its preparation include, by weight, 50 parts of alkoxysilyl modified polymer, 15 parts of plasticizer, 25 parts of filler, 7 parts of auxiliary agent and 3 parts of color paste.

[0047] The alkoxysilyl modified polymer is a dimethoxysilyl-terminated polyether, which is a combination of 13 Pa.s and 8 Pa.s at 25°C, with a weight ratio of 1:0.3; the dimethoxysilyl-terminated polyether with a viscosity of 13 Pa.s at 25°C was purchased from Japan's Kaneka Chemical, model S303H, and the dimethoxysilyl-terminated polyether with a viscosity of 8 Pa.s at 25°C was purchased from Japan's Kaneka Chemical, model S203H.

[0048] The plasticizer is polypropylene glycol with a molecular weight of 3000 Daltons, purchased from Wuhan Jixinyibang Biotechnology Co., Ltd.

[0049] The filler is a combination of light calcium carbonate and heavy calcium carbonate, with a weight ratio of 1.75:1; the particle size of the light calcium carbonate is 0.1 μm, and it is purchased from Guangdong Yongfeng Chemical Co., Ltd.

[0050] The auxiliary agent includes a mildew preventer, a thixotropic agent, a catalyst, and a coupling agent, with a weight ratio of 2:1:0.3:1; the mildew preventer is a combination of inorganic silver ions and zinc oxide, with a weight ratio of 1:1.5.

[0051] The coupling agent is a combination of diethylenetriaminopropyltrimethoxysilane and isopropyl tri(dioctylphosphoyl) titanate in a weight ratio of 1:1. The diethylenetriaminopropyltrimethoxysilane is purchased from Chenguang Chemical, and isopropyl tri(dioctylphosphoyl) titanate is purchased from Hangzhou Jessica Chemical Co., Ltd.

[0052] The catalyst is an organic zinc catalyst purchased from Shanghai Deyin Chemical Co., Ltd., model number DY-5350. The thixotropic agent is fumed silica.

[0053] A method for preparing an anti-mildew adhesive for external use in building construction comprises the following steps:

[0054] (1) Mix the alkoxysilane-modified polymer, plasticizer, mildew inhibitor, thixotropic agent and color paste in a vacuum mixture for 10 minutes;

[0055] (2) Then add the coupling agent and continue stirring the filler for 15 minutes;

[0056] (3) Finally, add the catalyst, stir for 5 minutes, discharge the material, and seal it.

[0057] Example 2

[0058] A mildew-proof adhesive for external use in building construction and a preparation method thereof. The specific steps are the same as those in Example 1, except that the alkoxysilyl-modified polymer is a dimethoxysilyl-terminated polyether having a viscosity of 13 Pa.s at 25°C.

[0059] Example 3

[0060] A mildew-proof glue for external use in building construction and a preparation method thereof. The specific steps are the same as those in Example 1, except that the filler is light calcium carbonate with a particle size of 0.1 μm.

[0061] Example 4

[0062] A mildew-proof adhesive for external use in building construction and a preparation method thereof. The specific steps are the same as those in Example 1, except that the coupling agent is diethylenetriaminopropyltrimethoxysilane.

[0063] Performance Testing

[0064] 1. Mildew resistance level: The mildew resistance level of the prepared mildew-proof glue is tested according to GB / T1741-2007 standard. The test bacteria are Aspergillus niger and Aspergillus flavus.

[0065] 2. Tensile strength: The tensile strength of the prepared anti-mildew glue was tested according to GB / T13477 standard.

[0066] 3. Elongation at break: The elongation at break of the mildew-proof adhesive prepared was tested according to GB / T13477 standard.

[0067] 4. Elastic recovery rate: The elastic recovery rate of the mildew-proof glue prepared is tested according to GB / T13477 standard.

[0068] Tested according to the above standards.

Claims

1. A mildew-proof adhesive for external use in building construction. It is characterized in that The raw materials for preparation include, by weight: 30-60 parts of alkoxysilane-modified polymer, 10-20 parts of plasticizer, 20-30 parts of filler, 5-10 parts of auxiliary agent, and 1-5 parts of color paste; The alkoxysilyl modified polymer is a dimethoxysilyl terminated polyether; the alkoxysilyl modified polymer is a combination of a viscosity of 13 Pa.s and 8 Pa.s at 25°C; The filler is a combination of light calcium carbonate and heavy calcium carbonate, and the particle size of the light calcium carbonate is 0.1-1 μm; The auxiliary agent is a combination of a mildew preventer, a thixotropic agent, a catalyst, and a coupling agent, and the mildew preventer is selected from one or a combination of metal ion mildew preventers, metal oxide mildew preventers, quaternary ammonium salt mildew preventers, biguanide mildew preventers, and thiazole mildew preventers; The coupling agent is a combination of diethylenetriaminopropyltrimethoxysilane and isopropyl tri(dioctylphosphoyloxy) titanate; the weight ratio of the diethylenetriaminopropyltrimethoxysilane to isopropyl tri(dioctylphosphoyloxy) titanate is 1:(0.5-1.5).

2. The anti-mildew adhesive for building construction according to claim 1, It is characterized in that The plasticizer is selected from one or a combination of aliphatic dibasic acid esters, fatty acid esters, polyol esters, phosphate plasticizers, alkyl sulfonates, fatty alcohols, and polyester plasticizers.

3. The anti-mildew adhesive for building construction according to claim 2, It is characterized in that The fatty alcohol is selected from one or a combination of n-hexanol, dodecanol, decanol, polyethylene glycol, polypropylene glycol, and palmityl alcohol, and the molecular weight of the polypropylene glycol is 2000-4000 Daltons.

4. The anti-mildew adhesive for building construction according to claim 1, It is characterized in that The catalyst is selected from one or a combination of organic tin catalysts, bismuth catalysts, organic zinc catalysts, and nitrogen heterocyclic olefin catalysts.

5. A method for preparing the anti-mildew adhesive for building construction according to any one of claims 1 to 4, It is characterized in that The following steps are involved: (1) Mix the alkoxysilane-modified polymer, plasticizer, mildew inhibitor, thixotropic agent and color paste in a vacuum mixture for 10-15 minutes; (2) Then add the coupling agent and continue stirring the filler for 10-15 minutes; (3) Finally, add the catalyst, stir for 5-10 minutes, discharge the material, and seal it.