Carbonyl sulfide hydrolysis catalyst and its preparation method and application

By preparing a carbonyl sulfur hydrolysis catalyst with a zinc-magnesium-aluminum composite oxide support, the problems of low activity and short lifespan of existing catalysts were solved, achieving high efficiency in carbonyl sulfur hydrolysis and resistance to chlorine poisoning, making it suitable for blast furnace gas desulfurization.

CN115869933BActive Publication Date: 2024-11-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111142765.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-28
Publication Date
2024-11-15
Estimated Expiration
2041-09-28

AI Technical Summary

Technical Problem

Existing carbonyl sulfur hydrolysis catalysts have unsatisfactory catalytic activity, short service life, and insufficient resistance to chlorine poisoning, making it difficult to effectively treat carbonyl sulfur in blast furnace gas.

Method used

Catalyst precursors were prepared using aluminum, zinc, magnesium, and alkali metal compounds. Through drying, calcination, and water washing, zinc-magnesium-aluminum composite oxide supports were formed, which improved the catalyst's resistance to chlorine poisoning and catalytic activity.

Benefits of technology

The prepared catalyst has a uniformly dispersed active component, high pore volume and specific surface area, which significantly improves catalytic activity and service life, especially exhibiting excellent carbonyl sulfur hydrolysis performance in a chlorine-containing atmosphere.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115869933B_ABST
    Figure CN115869933B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of gas purification, and specifically to a carbonyl sulfide hydrolysis catalyst and a preparation method and application thereof. The preparation method comprises: (1) subjecting an aluminum source, a zinc source, a magnesium source, an alkali metal compound and an auxiliary agent to a molding process to obtain a catalyst precursor; (2) drying and calcining the catalyst precursor in sequence to obtain a calcined product; (3) washing the calcined product with water and drying it to obtain a carbonyl sulfide hydrolysis catalyst. The active components can be evenly dispersed, the pore volume and specific surface area retention of the catalyst are high, and can be flexibly adjusted; the catalytic activity of the hydrolysis reaction is high, especially the resistance to chlorine poisoning is strong, and the service life is significantly improved; the preparation process is simple, which is conducive to energy saving and consumption reduction, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of gas purification, and in particular to a carbonyl sulfide hydrolysis catalyst and a preparation method and application thereof. Background Art

[0002] Blast furnace gas is one of the most important secondary energy sources for steel enterprises and has a wide range of uses. At present, steel mills generally use end-of-pipe treatment for desulfurization. The disadvantage is that the investment cost is high and it may not be able to fully meet the emission standards. Therefore, source control and blast furnace gas desulfurization are the most economical and convenient technical means for steel mills to manage. However, the technical difficulty of source control is relatively high, which is mainly related to the characteristics of blast furnace gas itself: 1. The composition of blast furnace gas is complex, and the main forms of sulfur element are carbonyl sulfide (COS), carbon disulfide, hydrogen sulfide, etc., among which organic sulfur (especially carbonyl sulfide) is the main one, accounting for more than 80%; 2. The gas volume is large, generally in the hundreds of thousands of standard cubic meters per hour; 3. There are many impurities. In addition to N 2 , CO 2 In addition to CO, it also contains water, dust, chlorine, etc. The above factors make blast furnace gas desulfurization face higher challenges.

[0003] The removal of carbonyl sulfide is the key to blast furnace gas desulfurization. The presence of carbonyl sulfide will not only cause problems such as catalyst poisoning and deactivation in subsequent production processes, and corrosion of production equipment and instruments, but more importantly, carbonyl sulfide discharged into the atmosphere without treatment will react with oxygen to form SO 2 , causing environmental pollution and harming health. At present, the mainstream process for removing carbonyl sulfide in industry is hydrolysis, which includes: firstly, hydrolyzing carbonyl sulfide into H 2 S, and then remove H by conventional desulfurization method 2 S, where the hydrolysis catalyst is the key. For carbonyl sulfide hydrolysis catalyst, alumina is usually used as a carrier. The prepared catalyst has the advantages of large specific surface area and convenient raw material source, but the hydrolysis product H 2 S and trace oxygen (O 2 ), water, dust, chlorine and other impurities will cause the activity of carbonyl sulfide hydrolysis catalyst to decrease rapidly or even become inactivated. Especially when the chlorine content in the feed gas is high, the poisoning of carbonyl sulfide hydrolysis catalyst is particularly serious. The current organic sulfur hydrolysis catalyst generally has a short life span and its catalytic activity needs to be improved.

[0004] Therefore, the development of highly active and long-life organic sulfur hydrolysis catalysts, especially hydrolysis catalysts with strong resistance to chlorine poisoning, is of great significance to the development of blast furnace gas desulfurization technology. Summary of the invention

[0005] The purpose of the present invention is to overcome the problems of the prior art organic sulfur hydrolysis catalysts, such as unsatisfactory catalytic activity, short service life and urgent need to improve the resistance to chlorine poisoning, and to provide a carbonyl sulfide hydrolysis catalyst and a preparation method and application thereof.

[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a carbonyl sulfide hydrolysis catalyst, comprising:

[0007] (1) subjecting an aluminum source, a zinc source, a magnesium source, an alkali metal compound and an additive to a molding process to obtain a catalyst precursor;

[0008] (2) drying and calcining the catalyst precursor in sequence to obtain a calcined product;

[0009] (3) washing the calcined product with water and drying it to obtain a carbonyl sulfide hydrolysis catalyst.

[0010] The second aspect of the present invention provides a carbonyl sulfide hydrolysis catalyst prepared by the method described in the first aspect.

[0011] The third aspect of the present invention provides use of the carbonyl sulfide hydrolysis catalyst described in the second aspect in blast furnace gas desulfurization.

[0012] Through the above technical solution, the method provided by the present invention has the following beneficial effects:

[0013] (1) The active components of the prepared carbonyl sulfide hydrolysis catalyst are evenly dispersed, the pore volume and specific surface area retention of the catalyst are high, and can be flexibly adjusted;

[0014] (2) The catalyst has high catalytic activity for the carbonyl sulfide hydrolysis reaction, especially strong resistance to hydrogen chloride poisoning. The catalyst is used to remove carbonyl sulfide from feed gas containing hydrogen chloride, and its service life is significantly longer. Compared with conventional hydrolysis catalysts, the service life can be basically increased by more than double;

[0015] (3) The preparation process is simple, which reduces the steps of loading the active components, and is beneficial to energy saving and cost reduction in the preparation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a device and process flow chart used in the carbonyl sulfide hydrolysis reaction test in the test example of the present invention.

[0017] Description of Reference Numerals

[0018] 1. Water and hydrochloric acid storage tanks 2. Reaction raw material sampling tanks 3. Reactor

[0019] 4. Reaction product sampling tank 5. Tail gas liquid alkali absorption tank DETAILED DESCRIPTION

[0020] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0021] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0022] The first aspect of the present invention provides a method for preparing a carbonyl sulfide hydrolysis catalyst, comprising:

[0023] (1) subjecting an aluminum source, a zinc source, a magnesium source, an alkali metal compound and an additive to a molding process to obtain a catalyst precursor;

[0024] (2) drying and calcining the catalyst precursor in sequence to obtain a calcined product;

[0025] (3) washing the calcined product with water and drying it to obtain a carbonyl sulfide hydrolysis catalyst.

[0026] According to the present invention, in the catalyst precursor, an aluminum source, a zinc source and a magnesium source are used to jointly form a carrier of the catalyst. By introducing magnesium and zinc alkaline oxides into alumina to form a zinc-magnesium-aluminum composite oxide carrier, the catalyst carrier's capacity to accommodate acidic harmful impurities such as hydrogen chloride is increased, and the active components of the catalyst are well protected. The carrier enables the catalyst to have a higher resistance to sulfur and oxygen poisoning, especially resistance to chlorine poisoning.

[0027] According to the present invention, preferably, the aluminum source can be selected from at least one of pseudo-boehmite, macroporous aluminum hydroxide and gibbsite, more preferably pseudo-boehmite, and further preferably high-purity pseudo-boehmite (ie, SB powder).

[0028] According to the present invention, preferably, the zinc source can be selected from at least one of zinc nitrate, zinc chloride and zinc oxide, more preferably zinc oxide;

[0029] According to the present invention, preferably, the magnesium source can be selected from at least one of magnesium nitrate, magnesium hydroxide and magnesium oxide, more preferably magnesium oxide.

[0030] According to the present invention, the alkali metal compound serves as an active component of the carbonyl sulfide hydrolysis catalyst and also acts as a pore expander, which can facilitate the formation of channels with larger pore sizes on the surface and inside of the carrier during the calcination of the catalyst precursor. The alkali metal compound is water-soluble or can react with water (the product of the reaction is soluble in water), can be dissolved in water and recovered in the form of an aqueous solution. Preferably, the alkali metal compound can be selected from alkali metal oxides and / or alkali metal carbonates, more preferably alkali metal carbonates. Preferably, the alkali metal is selected from potassium and / or sodium.

[0031] According to the present invention, the auxiliary agent can play a role of bonding and lubrication, which is conducive to the aluminum source, zinc source, magnesium source and alkali metal compound being molded together to obtain a catalyst precursor with high mechanical strength. The present invention has no particular limitation on the molding process, and conventional processes in the art can be used, including but not limited to extrusion molding, tablet molding, drop ball molding, rolling molding, etc. Preferably, the auxiliary agent can be selected from at least one of paraffin, graphite and methyl cellulose.

[0032] According to the present invention, in step (1), in order to obtain a carbonyl sulfide hydrolysis catalyst having high catalytic activity and resistance to chlorine poisoning, and at the same time being more conducive to the molding and processing of the raw materials, preferably, the aluminum source is Al 2 O 3 The weight ratio of aluminum source is (30-60): (5-20): (15-40): (5-25): (2-5), the weight ratio of zinc source is (30-60): (5-20): (15-40): (5-25): (2-5).

[0033] According to the present invention, in step (1), it is further preferred that the aluminum source is Al 2 O 3 In the embodiment of the present invention, the weight ratio of aluminum source:zinc source:magnesium source:alkali metal compound:auxiliary agent is (35-50):(8-15):(18-35):(8-20):(2-5), and a carbonyl sulfide hydrolysis catalyst with further improved catalytic activity and further enhanced chlorine poisoning resistance can be obtained. More preferably, the aluminum source is Al 2 O 3 The weight ratio of aluminum source: zinc source: magnesium source: alkali metal compound: additive is (38-45): (10-13): (23-30): (10-18): (3-4), and a carbonyl sulfide hydrolysis catalyst with higher catalytic activity and stronger resistance to chlorine poisoning can be obtained.

[0034] According to the present invention, in step (2), the drying can remove most of the organic solvent introduced in the catalyst precursor during the molding process or the pretreatment process of the raw materials before the molding process, so as to facilitate the subsequent calcination to obtain a catalyst product with better performance. Preferably, the drying conditions include: a temperature of 50-80°C and a time of 4-6 hours.

[0035] According to the present invention, in step (2), the calcination is divided into a first calcination and a second calcination which are carried out in sequence. The first calcination is carried out at a relatively low temperature, and the additive in the catalyst precursor is pyrolyzed and burned and removed in this process, and then the temperature is raised to carry out the second calcination, so that the catalyst precursor is further sintered and solidified to obtain a calcined product. Preferably, the conditions for the first calcination include: the temperature can be 450-600°C, and the time can be 0.5-2h; the conditions for the second calcination include: the temperature can be 800-1100°C, and the time can be 2-4h.

[0036] According to the present invention, in step (2), in order to obtain a carbonyl sulfide hydrolysis catalyst having higher catalytic activity and stronger resistance to chlorine poisoning, it is further preferred that the conditions for the first calcination include: the temperature can be 500-550°C, and the time can be 1-1.5h; the conditions for the second calcination include: the temperature can be 850-1000°C, and the time can be 2-3h.

[0037] According to the present invention, in step (3), after the calcined product is cooled to room temperature (in the present invention, room temperature refers to 0-40°C), it is washed with water. Part of the active components are dissolved in water and separated from the calcined product during the washing process. By controlling the degree of washing, the active component content and porosity of the carbonyl sulfide hydrolysis catalyst can be flexibly adjusted. The vacancies left after the part of the active components are separated from the carrier can make up for the catalyst specific surface area loss generated during the calcination process to a certain extent, so that the carbonyl sulfide hydrolysis catalyst obtained after calcination has a higher specific surface area retention. In the water washing treatment, deionized water is preferably used as washing water to rinse the calcined product. To further improve the elution efficiency, auxiliary equipment can also be used, including but not limited to atomizing nozzles. In order to achieve the effect of water washing, preferably, the weight ratio of washing water used in the water washing treatment: calcined product can be (2-10):1.

[0038] According to the present invention, in step (3), the calcined product after the water washing treatment is dried to remove water to obtain a carbonyl sulfide hydrolysis catalyst. Preferably, the drying conditions include: a temperature of 120-180° C. and a drying time of 2-4 hours.

[0039] According to the present invention, step (3) further comprises post-processing the washing liquid obtained after the water washing treatment to recover the alkali metal compound therein. The post-processing comprises sequential concentration and crystallization, filtration and separation, and optional drying and roasting. Specifically, when the alkali metal compound is an alkali metal carbonate, the alkali metal carbonate obtained can be recovered by sequentially concentrating and crystallizing the washing liquid and filtering and separating it; when the alkali metal compound is an alkali metal oxide, the crystal product obtained after filtering and separation needs to be dried and roasted to recover the alkali metal oxide obtained. The concentration and crystallization, filtration and separation, and drying and roasting can be carried out by conventional methods in the art, and the present invention has no particular limitation thereto. The recovered alkali metal compound can be combined with a fresh alkali metal compound and used together as an active component raw material to participate in step (1), or it can be used for other purposes.

[0040] According to the present invention, the method further comprises the following raw material pretreatment step before the molding process: first crushing and mixing the aluminum source, zinc source and magnesium source, and second crushing and mixing the obtained mixed powder with the alkali metal compound and the auxiliary agent to obtain a precursor powder. The precursor powder is subjected to the molding process to obtain the catalyst precursor.

[0041] According to the present invention, the first crushing and mixing and the second crushing and mixing can achieve sufficient breaking and mixing of the raw materials on the one hand, and can also obtain the mixed powder and precursor powder of suitable particle size on the other hand. By controlling the amount of the alkali metal compound in the raw material and the particle size of the mixed powder and precursor powder, the carbonyl sulfide hydrolysis catalyst can have a higher pore volume and a more optimized pore size distribution. Preferably, the average particle size of the mixed powder can be 0.1-8μm, and the average particle size of the precursor powder can be 0.1-5μm.

[0042] According to the present invention, the first crushing and mixing and the second crushing and mixing can be carried out by conventional methods in the art, and the present invention has no particular limitation thereto, as long as the raw materials can be fully mixed and the mixed powder and precursor powder in the above-mentioned particle size range can be obtained. For example, ball milling can be used, preferably a wet grinding process, wherein auxiliary reagents and materials such as a dispersion medium and a grinding medium, as well as process parameters such as a ball-to-material ratio, a mill speed, and a grinding time can be reasonably selected according to the particle size of the target product, and the present invention will not elaborate on this.

[0043] The second aspect of the present invention provides a carbonyl sulfide hydrolysis catalyst prepared by the method described in the first aspect.

[0044] According to the present invention, preferably, the pore volume of the carbonyl sulfide hydrolysis catalyst is 0.4-1.2 cm 3 / g, with a specific surface area of ​​40-240m2 / g.

[0045] The third aspect of the present invention provides use of the carbonyl sulfide hydrolysis catalyst described in the second aspect in blast furnace gas desulfurization.

[0046] The present invention will be described in detail below by way of examples. In the following examples and comparative examples,

[0047] The particle size test was carried out using a laser particle size analyzer, manufactured by Malvern Company, UK, model Mastersizer3000;

[0048] The specific surface area and pore volume of the catalyst were tested using a fully automatic nitrogen adsorption analyzer, the manufacturer of which was Quantachrome Instruments, Inc., USA, model AUTOSORB-1-C.

[0049] Example 1

[0050] (1) 41 parts by weight of SB powder (manufacturer: Sasol, Germany, Al 2 O 3 Calculated, Al in SB powder 2 O 3 The invention discloses a method for preparing a catalyst precursor comprising the steps of: placing 12 parts by weight of zinc oxide powder (calculated as ZnO, the content of ZnO in the zinc oxide powder is 99.5wt%), 26 parts by weight of magnesium oxide powder (calculated as MgO, the content of MgO in the magnesium oxide powder is 99.8wt%) in a ball mill, adding anhydrous ethanol as a dispersion medium, and cemented carbide balls as grinding media, setting the ball-to-material weight ratio to 15:1, and the mill speed to 220 rpm, and grinding for 10 hours to obtain a mixed powder with an average particle size of 1.5 μm; then continuing to add 17.5 parts by weight of anhydrous potassium carbonate and 3.5 parts by weight of paraffin, and supplementing an appropriate amount of anhydrous ethanol as a dispersion medium to keep the material fully moistened, adjusting the mill speed to 120 rpm, and grinding for 12 hours to obtain a precursor powder with an average particle size of 0.8 μm; extruding the above precursor powder to obtain a catalyst precursor;

[0051] (2) drying the catalyst precursor obtained in step (1) at 60° C. for 5 h, then heating to 550° C. for a first calcination for 1.5 h, and then further heating to 900° C. for a second calcination for 2.5 h to obtain a calcined product;

[0052] (3) After the calcined product obtained in step (2) is cooled to room temperature, it is rinsed with deionized water (the weight ratio of deionized water to calcined product is 5:1), and then dried at 150° C. for 2 hours to obtain a carbonyl sulfide hydrolysis catalyst (denoted as S1); wherein the washing liquid obtained after eluting is concentrated, crystallized, filtered and separated to recover potassium carbonate therein.

[0053] The pore volume of S1 is 0.85 cm 3 / g, specific surface area is 205m 2 / g.

[0054] Example 2

[0055] (1) 50 parts by weight of SB powder (in the form of Al 2 O 3 Calculated, Al in SB powder 2 O 3 The invention discloses a method for preparing a catalyst precursor comprising the steps of: placing 14 parts by weight of zinc oxide powder (calculated as ZnO, the content of ZnO in the zinc oxide powder is 99.5wt%), 22 parts by weight of magnesium oxide powder (calculated as MgO, the content of MgO in the magnesium oxide powder is 99.8wt%) in a ball mill, adding anhydrous ethanol as a dispersion medium, and cemented carbide balls as grinding media, setting the ball-to-material weight ratio to 15:1, and the mill speed to 200 rpm, and grinding for 12 hours to obtain a mixed powder with an average particle size of 1.6μm; then continuing to add 9 parts by weight of anhydrous potassium carbonate and 5 parts by weight of paraffin, and supplementing an appropriate amount of anhydrous ethanol as a dispersion medium to keep the material fully moistened, adjusting the mill speed to 150 rpm, and grinding for 12 hours to obtain a precursor powder with an average particle size of 0.7μm; extruding the above precursor powder to obtain a catalyst precursor;

[0056] (2) drying the catalyst precursor obtained in step (1) at 60° C. for 5 h, then heating to 550° C. for a first calcination for 1.5 h, and then further heating to 900° C. for a second calcination for 2.5 h to obtain a calcined product;

[0057] (3) After the calcined product obtained in step (2) is cooled to room temperature, it is rinsed with deionized water (the weight ratio of deionized water to calcined product is 3.5:1), and then dried at 150° C. for 2 hours to obtain a carbonyl sulfide hydrolysis catalyst (denoted as S2); wherein the washing liquid obtained after eluting is concentrated, crystallized, filtered and separated to recover potassium carbonate therein.

[0058] The pore volume of S2 is 0.53 cm 3 / g, specific surface area is 175m 2 / g

[0059] Example 3

[0060] (1) 48 parts by weight of SB powder (in the form of Al 2 O 3 Calculated, Al in SB powder 2 O 3The invention discloses a method for preparing a catalyst precursor comprising the steps of: placing 9 parts by weight of zinc oxide powder (calculated as ZnO, the content of ZnO in the zinc oxide powder is 75.2wt%), 9 parts by weight of zinc oxide powder (calculated as ZnO, the content of ZnO in the zinc oxide powder is 99.5wt%), and 31 parts by weight of magnesium oxide powder (calculated as MgO, the content of MgO in the magnesium oxide powder is 99.8wt%) in a ball mill, adding anhydrous ethanol as a dispersion medium, and cemented carbide balls as grinding media, setting the ball-to-material weight ratio to 15:1, and the mill speed to 220 rpm, and grinding for 10 hours to obtain a mixed powder with an average particle size of 1.5μm; then continuing to add 9.5 parts by weight of anhydrous potassium carbonate and 2.5 parts by weight of paraffin, and supplementing an appropriate amount of anhydrous ethanol as a dispersion medium to keep the material fully moistened, adjusting the mill speed to 120 rpm, and grinding for 10 hours to obtain a precursor powder with an average particle size of 0.9μm; extruding the above precursor powder to obtain a catalyst precursor;

[0061] (2) drying the catalyst precursor obtained in step (1) at 60° C. for 5 h, then heating to 550° C. for a first calcination for 1.5 h, and then further heating to 900° C. for a second calcination for 2.5 h to obtain a calcined product;

[0062] (3) After the calcined product obtained in step (2) is cooled to room temperature, it is rinsed with deionized water (the weight ratio of deionized water to calcined product is 4:1), and then dried at 150° C. for 2 hours to obtain a carbonyl sulfide hydrolysis catalyst (denoted as S3); wherein the washing liquid obtained after eluting is concentrated, crystallized, filtered and separated to recover potassium carbonate therein.

[0063] The pore volume of S3 is 0.62 cm 3 / g, specific surface area is 183m 2 / g.

[0064] Example 4

[0065] (1) 48 parts by weight of pseudo-boehmite powder (in the form of Al 2 O 3 The Al content in boehmite powder is calculated. 2 O 3The invention discloses a method for preparing a catalyst precursor comprising the steps of: placing 9 parts by weight of zinc oxide powder (calculated as ZnO, the content of ZnO in the zinc oxide powder is 62.5wt%), 9 parts by weight of zinc oxide powder (calculated as ZnO, the content of ZnO in the zinc oxide powder is 99.5wt%), and 31 parts by weight of magnesium oxide powder (calculated as MgO, the content of MgO in the magnesium oxide powder is 99.8wt%) in a ball mill, adding anhydrous ethanol as a dispersion medium, and cemented carbide balls as grinding media, setting the ball-to-material weight ratio to 15:1, and the mill speed to 220 rpm, and grinding for 10 hours to obtain a mixed powder with an average particle size of 1.5μm; then continuing to add 9.5 parts by weight of anhydrous potassium carbonate and 2.5 parts by weight of paraffin wax, and supplementing an appropriate amount of anhydrous ethanol as a dispersion medium to keep the material fully moistened, adjusting the mill speed to 120 rpm, and grinding for 10 hours to obtain a precursor powder with an average particle size of 0.9μm; extruding the above precursor powder to obtain a catalyst precursor;

[0066] (2) drying the catalyst precursor obtained in step (1) at 60° C. for 5 h, then heating to 550° C. for a first calcination for 1.5 h, and then further heating to 900° C. for a second calcination for 2.5 h to obtain a calcined product;

[0067] (3) After the calcined product obtained in step (2) is cooled to room temperature, it is rinsed with deionized water (the weight ratio of deionized water to calcined product is 4:1), and then dried at 150° C. for 2 hours to obtain a carbonyl sulfide hydrolysis catalyst (denoted as S4); wherein the washing liquid obtained after eluting is concentrated, crystallized, filtered and separated to recover potassium carbonate therein.

[0068] The pore volume of S4 is 0.58 cm 3 / g, specific surface area is 179m 2 / g.

[0069] Example 5

[0070] (1) 48 parts by weight of SB powder (in the form of Al 2 O 3 Calculated, Al in SB powder 2 O 3The invention discloses a method for preparing a catalyst precursor comprising the steps of: placing 9 parts by weight of zinc nitrate powder (calculated as ZnO, the ZnO content in the zinc nitrate powder is 75.2wt%), 9 parts by weight of zinc nitrate powder (calculated as ZnO, the ZnO content in the zinc nitrate powder is 42.5wt%), and 31 parts by weight of magnesium oxide powder (calculated as MgO, the MgO content in the magnesium oxide powder is 99.8wt%) in a ball mill, adding anhydrous ethanol as a dispersion medium, and cemented carbide balls as grinding media, setting the ball-to-material weight ratio to 15:1, and the mill speed to 220 rpm, and grinding for 10 hours to obtain a mixed powder with an average particle size of 1.5μm; then continuing to add 9.5 parts by weight of anhydrous potassium carbonate and 2.5 parts by weight of paraffin wax, and supplementing an appropriate amount of anhydrous ethanol as a dispersion medium to keep the material fully moistened, adjusting the mill speed to 120 rpm, and grinding for 10 hours to obtain a precursor powder with an average particle size of 0.9μm; extruding the above precursor powder to obtain a catalyst precursor;

[0071] (2) drying the catalyst precursor obtained in step (1) at 60° C. for 5 h, then heating to 550° C. for a first calcination for 1.5 h, and then further heating to 900° C. for a second calcination for 2.5 h to obtain a calcined product;

[0072] (3) After the calcined product obtained in step (2) is cooled to room temperature, it is rinsed with deionized water (the weight ratio of deionized water to calcined product is 4:1), and then dried at 150° C. for 2 hours to obtain a carbonyl sulfide hydrolysis catalyst (denoted as S5); wherein the washing liquid obtained after eluting is concentrated, crystallized, filtered and separated to recover potassium carbonate therein.

[0073] The pore volume of S5 is 0.65 cm 3 / g, specific surface area is 188m 2 / g.

[0074] Example 6

[0075] (1) 48 parts by weight of SB powder (in the form of Al 2 O 3 Calculated, Al in SB powder 2 O 3The invention discloses a method for preparing a catalyst precursor comprising the steps of: placing 9 parts by weight of zinc oxide powder (calculated as ZnO, the ZnO content in the zinc oxide powder is 75.2wt%), 9 parts by weight of zinc oxide powder (calculated as ZnO, the ZnO content in the zinc oxide powder is 99.5wt%), and 31 parts by weight of magnesium hydroxide powder (calculated as MgO, the MgO content in the magnesium hydroxide powder is 66.8wt%) in a ball mill, adding anhydrous ethanol as a dispersion medium, and cemented carbide balls as grinding media, setting the ball-to-material weight ratio to 15:1, and the mill speed to 220 rpm, and grinding for 10 hours to obtain a mixed powder with an average particle size of 1.5μm; then continuing to add 9.5 parts by weight of anhydrous potassium carbonate and 2.5 parts by weight of paraffin wax, and supplementing an appropriate amount of anhydrous ethanol as a dispersion medium to keep the material fully moistened, adjusting the mill speed to 120 rpm, and grinding for 10 hours to obtain a precursor powder with an average particle size of 0.9μm; extruding the above precursor powder to obtain a catalyst precursor;

[0076] (2) drying the catalyst precursor obtained in step (1) at 60° C. for 5 h, then heating to 550° C. for a first calcination for 1.5 h, and then further heating to 900° C. for a second calcination for 2.5 h to obtain a calcined product;

[0077] (3) After the calcined product obtained in step (2) is cooled to room temperature, it is rinsed with deionized water (the weight ratio of deionized water to calcined product is 4:1), and then dried at 150° C. for 2 hours to obtain a carbonyl sulfide hydrolysis catalyst (denoted as S6); wherein the washing liquid obtained after eluting is concentrated, crystallized, filtered and separated to recover potassium carbonate therein.

[0078] The pore volume of S6 is 0.59 cm 3 / g, specific surface area is 174m 2 / g.

[0079] Example 7

[0080] (1) 48 parts by weight of SB powder (in the form of Al 2 O 3 Calculated, Al in SB powder 2 O 3The invention discloses a method for preparing a catalyst precursor comprising the steps of: placing 9 parts by weight of zinc oxide powder (calculated as ZnO, the content of ZnO in the zinc oxide powder is 75.2wt%), 9 parts by weight of zinc oxide powder (calculated as ZnO, the content of ZnO in the zinc oxide powder is 99.5wt%), and 31 parts by weight of magnesium oxide powder (calculated as MgO, the content of MgO in the magnesium oxide powder is 99.8wt%) in a ball mill, adding anhydrous ethanol as a dispersion medium, and cemented carbide balls as grinding media, setting the ball-to-material weight ratio to 15:1, and the mill speed to 220 rpm, and grinding for 10 hours to obtain a mixed powder with an average particle size of 1.5μm; then continuing to add 9.5 parts by weight of anhydrous sodium carbonate and 2.5 parts by weight of paraffin, and supplementing an appropriate amount of anhydrous ethanol as a dispersion medium to keep the material fully moistened, adjusting the mill speed to 120 rpm, and grinding for 10 hours to obtain a precursor powder with an average particle size of 0.9μm; extruding the above precursor powder to obtain a catalyst precursor;

[0081] (2) drying the catalyst precursor obtained in step (1) at 60° C. for 5 h, then heating to 550° C. for a first calcination for 1.5 h, and then further heating to 900° C. for a second calcination for 2.5 h to obtain a calcined product;

[0082] (3) After the calcined product obtained in step (2) is cooled to room temperature, it is rinsed with deionized water (the weight ratio of deionized water to calcined product is 4:1), and then dried at 150° C. for 2 hours to obtain a carbonyl sulfide hydrolysis catalyst (denoted as S7); wherein the washing liquid obtained after eluting is concentrated, crystallized, filtered and separated to recover the sodium carbonate therein.

[0083] The pore volume of S7 is 0.64 cm 3 / g, specific surface area is 185m 2 / g.

[0084] Comparative Example 1

[0085] The method of Example 1 is followed, except that in step (1), instead of using a zinc source and a magnesium source, 79 parts by weight of SB powder (in the form of Al 2 O 3 Calculated, Al in SB powder 2 O 3 The content is 75.2 wt%), and other conditions are the same as those in Example 1. A catalyst (denoted as D1) is obtained.

[0086] The pore volume of D1 is 0.88 cm 3 / g, specific surface area is 203m 2 / g.

[0087] Comparative Example 2

[0088] The method of Example 1 is followed, except that the amounts of the raw materials in step (1) are as follows: 25 parts by weight of SB powder (in the form of Al 2O 3 Calculated, Al in SB powder 2 O 3 The catalyst (denoted as D2) was prepared by mixing 25 parts by weight of zinc oxide powder (calculated as ZnO, the ZnO content in the zinc oxide powder was 99.5wt%), 10 parts by weight of magnesium oxide powder (calculated as MgO, the MgO content in the magnesium oxide powder was 99.8wt%), 30 parts by weight of anhydrous potassium carbonate and 10 parts by weight of paraffin. Other conditions were the same as those in Example 1.

[0089] The pore volume of D2 is 0.52 cm 3 / g, specific surface area is 165m 2 / g.

[0090] Comparative Example 3

[0091] The method of Example 1 was followed, except that the grinding time of the aluminum source, zinc source and magnesium source in step (1) was 2 hours, and a mixed powder with an average particle size of 23.5 μm was obtained; the grinding time of the mixed material with anhydrous potassium carbonate and paraffin was 2 hours, and a precursor powder with an average particle size of 15.5 μm was obtained. Other conditions were the same as those of Example 1. A catalyst (denoted as D3) was obtained.

[0092] The pore volume of D3 is 0.44 cm 3 / g, specific surface area is 103m 2 / g.

[0093] Comparative Example 4

[0094] The method of Example 1 is followed, except that the water washing treatment of the calcined product is omitted in step (3), and the product is directly dried. The other conditions are the same as those of Example 1. A catalyst (denoted as D4) is obtained.

[0095] The pore volume of D4 is 0.32 cm 3 / g, specific surface area is 88m 2 / g.

[0096] Comparative Example 5

[0097] (1) Select macroporous pseudo-boehmite (producer: Shandong Aluminum Company, Al 2 O 3 The Al content in macroporous pseudo-boehmite is 2 O 3 The strip alumina prepared from the precursor with a content of 65.3 wt %) was used as a carrier (the pore volume of the strip alumina carrier was 0.68 cc / g and the specific surface area was 205 m 2 / g, bulk density of 0.38 kg / L); 500 grams of the above carrier was placed in a 2L container and supersaturated with a 15wt% potassium carbonate aqueous solution, the immersion temperature was controlled to be 65 ° C, and the immersion time was 60 minutes;

[0098] (2) The product impregnated in step (1) was centrifuged and filtered to remove excess impregnation liquid, and then the separated solid was dried at 150° C. for 2 h to obtain a catalyst (denoted as D5).

[0099] The pore volume of D5 is 0.42 cm 3 / g, specific surface area is 168m 2 / g.

[0100] Test Case

[0101] The catalysts (S1-S7, D1-D5) prepared in Examples 1-7 and Comparative Examples 1-5 were used in a carbonyl sulfide hydrolysis reaction test to evaluate the hydrolysis catalytic activity, resistance to hydrogen chloride poisoning and service life of the catalysts.

[0102] The equipment and process flow used in the test are as follows: Figure 1 As shown, specifically:

[0103] Raw gas composition: COS content is 120mg / m 3 ;CO 2 The volume fraction is 19%; H 2 The volume fraction of O (water vapor) is 3%; the content of HCl is 300120 mg / m 3 ; The rest is N 2 (Note: N 2 As carrier gas, N 2 The feed gas is introduced with H through a water tank containing 3 wt% hydrochloric acid. 2 O and HCl).

[0104] The catalytic reaction conditions are: mass space velocity of raw gas: 10h -1 , pressure: 2.5 bar, temperature: 100°C; gas chromatography (Jelen 7890A, detector FPD) was used to determine the COS content at the inlet and outlet of the evaluation device after different reaction times, and the COS conversion rate was used to characterize the hydrolysis catalytic activity, tolerance to hydrogen chloride poisoning and service life of the above-mentioned catalyst, wherein the COS conversion rate was calculated according to formula (I), and the results are shown in Table 1.

[0105]

[0106] In formula (I), M 0 、M 1 represent the volume concentration of COS at the inlet and outlet, respectively.

[0107] Table 1

[0108]

[0109] As can be seen from Table 1, the carbonyl sulfide hydrolysis catalysts S1-S7 provided by the present invention have excellent COS hydrolysis catalytic activity and high COS conversion rate. As the reaction time increases, although the COS conversion rate shows a gradually decreasing trend, the decrease is very low. After the reaction is carried out for 120 hours, the COS conversion rate is still higher than 70%, which indicates that the carbonyl sulfide hydrolysis catalyst provided by the present invention has good tolerance to hydrogen chloride poisoning and a longer service life.

[0110] In particular, Comparative Example 1 uses a single alumina as a catalyst carrier, which cannot effectively protect the active components of the catalyst. Comparative Example 2 does not use the catalyst component formula of the present invention, resulting in a low initial activity of the catalyst, and the COS conversion rate and resistance to hydrogen chloride poisoning performance cannot reach the effects of S1-S7.

[0111] In Comparative Example 3, the particle size of the mixed powder and the precursor powder is relatively large, resulting in uneven dispersion of the active components of the catalyst, which greatly affects the COS hydrolysis catalytic activity of the catalyst; in Comparative Example 4, the calcined product was not washed with water, resulting in a smaller catalyst pore volume and specific surface area, and the COS conversion rate and tolerance to hydrogen chloride poisoning were worse than those of S1-S7.

[0112] In Comparative Example 5, an alumina-based organic sulfur hydrolysis catalyst was prepared by a conventional impregnation method. The catalyst was rapidly poisoned after contacting hydrogen chloride during the reaction, resulting in a significant decrease in the catalytic activity for COS hydrolysis. The COS conversion rate decreased significantly with the extension of the reaction time, and the service life was reached after 48 hours of reaction (according to the use requirements, the catalyst is usually considered to be deactivated when the COS conversion rate is lower than 80%). The COS hydrolysis catalytic activity, tolerance to hydrogen chloride poisoning and service life are far inferior to those of S1-S7.

[0113] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing a carbonyl sulfide hydrolysis catalyst, characterized in that: include: (1) forming an aluminum source, a zinc source, a magnesium source, an alkali metal compound and an additive to obtain a catalyst precursor; (2) drying and calcining the catalyst precursor in sequence to obtain a calcined product; (3) washing the calcined product with water and drying it to obtain a carbonyl sulfide hydrolysis catalyst; The aluminum source is calculated as Al2O3, the zinc source is calculated as ZnO, and the magnesium source is calculated as MgO. The weight ratio of the aluminum source: the zinc source: the magnesium source: the alkali metal compound: the auxiliary agent is (30-60): (5-20): (15-40): (5-25): (2-5); the auxiliary agent is selected from at least one of paraffin, graphite and methyl cellulose; Before the molding process, the following steps are performed: the aluminum source, zinc source and magnesium source are first crushed and mixed, and the obtained mixed powder is second crushed and mixed with the alkali metal compound and the additive to obtain a precursor powder; the average particle size of the mixed powder is 0.1-8μm, and the average particle size of the precursor powder is 0.1-5μm.

2. The method according to claim 1, wherein: The aluminum source is selected from at least one of pseudo-boehmite, macroporous aluminum hydroxide and gibbsite; The zinc source is selected from at least one of zinc nitrate, zinc chloride and zinc oxide; The magnesium source is selected from at least one of magnesium nitrate, magnesium hydroxide and magnesium oxide.

3. The method according to claim 2, wherein: The aluminum source is pseudo-boehmite; the zinc source is zinc oxide; and the magnesium source is magnesium oxide.

4. The method according to any one of claims 1 to 3, wherein: The alkali metal compound is selected from alkali metal oxides and / or alkali metal carbonates.

5. The method according to claim 4, wherein: The alkali metal compound is an alkali metal carbonate.

6. The method according to claim 5, wherein: The alkali metal is selected from potassium and / or sodium.

7. The method according to claim 1, wherein: The aluminum source is calculated as Al2O3, the zinc source is calculated as ZnO, and the magnesium source is calculated as MgO. The weight ratio of the aluminum source: zinc source: magnesium source: alkali metal compound: additive is (35-50): (8-15): (18-35): (8-20): (2-5).

8. The method according to claim 7, wherein: The aluminum source is calculated as Al2O3, the zinc source is calculated as ZnO, and the magnesium source is calculated as MgO. The weight ratio of the aluminum source: zinc source: magnesium source: alkali metal compound: additive is (38-45): (10-13): (23-30): (10-18): (3-4).

9. The method according to any one of claims 1-3, 5-8, wherein: In step (2), the drying conditions include: temperature of 50-80° C. and time of 4-6 hours.

10. The method according to claim 4, wherein: In step (2), the drying conditions include: temperature of 50-80° C. and time of 4-6 hours.

11. The method according to any one of claims 1-3, 5-8, and 10, wherein: In step (2), the roasting is divided into a first roasting and a second roasting which are performed sequentially; The first calcination conditions include: temperature of 450-600°C and time of 0.5-2h; The second calcination conditions include: temperature of 800-1100° C. and time of 2-4 hours.

12. The method according to claim 4, wherein: In step (2), the roasting is divided into a first roasting and a second roasting which are performed sequentially; The first calcination conditions include: temperature of 450-600°C and time of 0.5-2h; The second calcination conditions include: temperature of 800-1100° C. and time of 2-4 hours.

13. The method according to claim 9, wherein: In step (2), the roasting is divided into a first roasting and a second roasting which are performed sequentially; The first calcination conditions include: temperature of 450-600°C and time of 0.5-2h; The second calcination conditions include: temperature of 800-1100° C. and time of 2-4 hours.

14. The method according to claim 11, wherein the first calcination conditions include: The temperature is 500-550℃, and the time is 1-1.5h; The second calcination conditions include: temperature of 850-1000° C. and time of 2-3 hours.

15. The method according to claim 12 or 13, wherein the first calcination conditions include: The temperature is 500-550℃, and the time is 1-1.5h; The second calcination conditions include: temperature of 850-1000° C. and time of 2-3 hours.

16. The method according to any one of claims 1-3, 5-8, 10, 12-14, wherein: In step (3), the weight ratio of washing water used in the water washing treatment to the roasted product is (2-10):1; And / or, the drying conditions include: temperature of 120-180° C. and time of 2-4 hours.

17. The method according to claim 4, wherein: In step (3), the weight ratio of washing water used in the water washing treatment to the roasted product is (2-10):1; And / or, the drying conditions include: temperature of 120-180° C. and time of 2-4 hours.

18. The method according to claim 9, wherein: In step (3), the weight ratio of washing water used in the water washing treatment to the roasted product is (2-10):1; And / or, the drying conditions include: temperature of 120-180° C. and time of 2-4 hours.

19. The method according to claim 11, wherein: In step (3), the weight ratio of washing water used in the water washing treatment to the roasted product is (2-10):1; And / or, the drying conditions include: temperature of 120-180° C. and time of 2-4 hours.

20. The method according to claim 15, wherein: In step (3), the weight ratio of washing water used in the water washing treatment to the roasted product is (2-10):1; And / or, the drying conditions include: temperature of 120-180° C. and time of 2-4 hours.

21. The method according to claim 16, wherein: Step (3) also includes post-treating the washing liquid obtained after the water washing treatment to recover the alkali metal compound therein.

22. The method according to any one of claims 17 to 20, wherein: Step (3) also includes post-treating the washing liquid obtained after the water washing treatment to recover the alkali metal compound therein.

23. A carbonyl sulfide hydrolysis catalyst prepared by the method according to any one of claims 1 to 22.

24. The carbonyl sulfide hydrolysis catalyst according to claim 23, wherein the pore volume of the catalyst is 0.4-1.2 cm 3 / g, with a specific surface area of ​​40-240m 2 / g.

25. Use of the carbonyl sulfide hydrolysis catalyst according to claim 23 or 24 in blast furnace gas desulfurization.