Process for removing high-temperature deposited silicon, oxygen, titanium nitride and fluoride films on the surface of the electrostatic adsorption disk of semiconductor etching equipment ESC

A comprehensive cleaning process for ESC electrostatic adsorption disks in semiconductor etching equipment removes high-temperature films, addressing cost and waste issues by preserving the component and achieving cleanliness for reuse.

CN115870276BActive Publication Date: 2024-12-03FERROTEC TECH&DEV(DALIAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211434358.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-16
Publication Date
2024-12-03
Estimated Expiration
2042-11-16

AI Technical Summary

Technical Problem

The frequent replacement of ESC electrostatic adsorption disks in semiconductor etching equipment due to deposited films leads to high costs and resource waste, necessitating an effective cleaning and refurbishment process that protects the component body and ensures cleanliness for microenvironment use.

Method used

A multi-step process involving protective taping, immersion in pure water, use of specific chemical solutions, rinsing, wiping, grinding, polishing, helium hole flushing, ultrasonic cleaning, and final drying to remove silicon, oxygen, titanium nitride, and fluoride films from the ESC electrostatic adsorption disk.

Benefits of technology

The process effectively removes high-temperature deposited films while preserving the component, reducing costs by 1/80 to 1/100 of new component prices and ensuring the surface meets equipment cavity requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115870276B_ABST
    Figure CN115870276B_ABST
Patent Text Reader

Abstract

The invention discloses a process for removing silicon, oxygen, titanium nitride and fluoride deposited films deposited at high temperature on the surface of an ESC electrostatic adsorption disk of a semiconductor etching device, comprising protecting the non-cleaning part of the ESC electrostatic adsorption disk with an acid-alkali-resistant tape; then putting it in pure water; then soaking it in a mixed acid solution A; after rinsing, dipping the mixed solution B to wipe the ceramic surface; after rinsing, dipping the mixed solution C to wipe the ceramic surface; after rinsing, turning the ESC electrostatic adsorption disk upside down and soaking it in a mixed solution D; after rinsing, removing part of the acid-alkali-resistant tape; connecting pure water to rinse the helium hole; polishing; stopping the pure water rinse of the helium hole; dipping the mixed solution E to wipe the ceramic surface of the ESC electrostatic adsorption disk; and then performing subsequent ultrasonic cleaning and drying. This process removes the silicon, oxygen, titanium nitride and fluoride residual films that have been deposited on the surface while fully protecting the component body from corrosion and loss, and effectively removes the color film on the surface caused by the high temperature of the machine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of cleaning and renovation of key components of semiconductor precision equipment, and in particular to a process for removing silicon, oxygen, titanium nitride and fluoride deposited films deposited at high temperature on the surface of an ESC electrostatic adsorption disk of a semiconductor etching device. Background Art

[0002] Semiconductor plasma etching (Plasma Dry ETCH) is the most common form of dry etching. Its principle is that the corrosive gas exposed to the electronic area forms plasma. The resulting ionized gas and the gas composed of released high-energy electrons form plasma. The ionized gas atoms are accelerated by the electric field to bombard the chip surface, so that the atoms or molecules on the chip surface contact and react with the active atoms in the plasma atmosphere to form gaseous products and leave the crystal surface to cause etching; the ESC electrostatic adsorption disk is the only core component that contacts the chip when the equipment cavity reacts. Its structure is complex and expensive.

[0003] Since the chamber of the semiconductor etching equipment will continuously deposit various gas molecules on the surface of the ESC electrostatic adsorption disk during reaction, the ESC electrostatic adsorption disk components need to be replaced regularly. If new components are replaced every time, it will increase huge costs for semiconductor manufacturing companies and waste resources. Therefore, the cleaning and refurbishment process is of great significance for the recycling of the components. Summary of the invention

[0004] The purpose of the present invention is to provide a process for removing silicon, oxygen, titanium nitride and fluoride deposited films deposited at high temperature on the surface of the electrostatic adsorption disk of the semiconductor etching equipment ESC. The process removes the silicon, oxygen, titanium nitride and fluoride deposited films deposited on the surface while fully protecting the component body from corrosion and loss, making the surface absolutely clean and able to meet the microenvironment use requirements in the equipment cavity.

[0005] To achieve the above purpose, the present application proposes a process for removing silicon, oxygen, titanium nitride and fluoride deposited films deposited at high temperature on the surface of the electrostatic adsorption disk of the semiconductor etching equipment ESC, including:

[0006] Step 1: Protect the electrode holes and helium holes on the back of the ESC electrostatic adsorption disk with acid- and alkali-resistant tape, and then protect the entire back and sides with acid- and alkali-resistant tape;

[0007] Step 2: Immerse the protected ESC electrostatic adsorption plate in 55°-65° pure water for a period of time, and bubble and stir the pure water during the immersion period;

[0008] Step 3: prepare mixed solution A;

[0009] Step 4: Take out the ESC electrostatic adsorption plate from the pure water, drain the remaining liquid, and soak it in the mixed acid solution A for 3 to 4 hours;

[0010] Step 5: Take out the ESC electrostatic adsorption plate from the mixed solution A and rinse it with an air-water gun at a pressure of 0.4-0.5 MPa;

[0011] Step 6: Prepare mixed solution B;

[0012] Step 7: After rinsing, use a dust-free cloth to dip in mixed solution B and wipe the ceramic surface of the ESC electrostatic adsorption plate;

[0013] Step 8: After wiping, use an air-water gun to rinse the ceramic surface of the ESC electrostatic adsorption plate at a pressure of 0.4-0.5 MPa;

[0014] Step 9: Prepare mixed solution C;

[0015] Step 10: After rinsing, use a dust-free cloth to dip in mixed solution C and wipe the ceramic surface of the ESC electrostatic adsorption plate;

[0016] Step 11: After wiping, use an air-water gun to rinse the ceramic surface of the ESC electrostatic adsorption plate at a pressure of 0.4-0.5 MPa;

[0017] Step 12: prepare mixed solution D;

[0018] Step 13: After rinsing, place the ESC electrostatic adsorption plate upside down and soak it in the mixed solution D for a period of time;

[0019] Step 14: After soaking, use an air-water gun to rinse the ceramic surface of the ESC electrostatic adsorption plate at a pressure of 0.4-0.5 MPa;

[0020] Step 15: After rinsing, remove the acid- and alkali-resistant tape on the back and sides of the whole, and also remove the acid- and alkali-resistant tape on the helium hole;

[0021] Step 16: Use an air-water gun to flush the entire ESC electrostatic adsorption plate at a pressure of 0.4-0.5 MPa;

[0022] Step 17: Install the helium hole flushing and purge fixture of the ESC electrostatic adsorption plate, and connect pure water to flush the helium hole. The flushing pressure is 0.1-0.2 MPa;

[0023] Step 18: Use a diamond grinding disc to grind the ceramic surface of the ESC electrostatic adsorption disk, and keep flushing the helium hole with pure water until the grinding is completed;

[0024] Step 19: Use an air-water gun to flush the entire ESC electrostatic adsorption plate at a pressure of 0.4-0.5 MPa;

[0025] Step 20: Stop flushing the helium hole with pure water and remove the ESC electrostatic adsorption plate from the fixture;

[0026] Step 21: Use an industrial sponge to polish the anodized surface on the side and back of the ESC electrostatic adsorption plate;

[0027] Step 22: After polishing, use an air-water gun to rinse the entire ESC electrostatic adsorption plate at a pressure of 0.4-0.5 MPa;

[0028] Step 23: After rinsing, use a high-purity nitrogen gun to dry the moisture on the surface of the ESC electrostatic adsorption plate and in the helium holes;

[0029] Step 24: Protect the back and sides of the ESC electrostatic adsorption plate with acid- and alkali-resistant tape;

[0030] Step 25: preparing mixed solution E;

[0031] Step 26: Use a dust-free cloth to dip in the mixed solution E and wipe the ceramic surface of the ESC electrostatic adsorption plate;

[0032] Step 27: After wiping, use an air-water gun to rinse the ceramic surface of the ESC electrostatic adsorption plate at a pressure of 0.4-0.5 MPa;

[0033] Step 28: After rinsing, remove the acid-alkali resistant tape on the back and sides of the ESC electrostatic adsorption plate;

[0034] Step 29: Use an air-water gun to flush the entire ESC electrostatic adsorption plate at a flushing pressure of 0.4-0.5 MPa;

[0035] Step 30: Use ultrasonic waves to clean the ESC electrostatic adsorption plate;

[0036] Step 31: After ultrasonic cleaning, remove the acid-alkali resistant tape from the electrode holes on the back of the ESC electrostatic adsorption disk;

[0037] Step 32: Dry the ESC electrostatic adsorption plate.

[0038] Furthermore, the mixed solution A is prepared by mixing ammonia water, hydrogen peroxide and pure water in a ratio of 2:3:5.

[0039] Furthermore, the mixed solution B is prepared by mixing ammonia water, hydrogen peroxide and pure water in a ratio of 1:3:6.

[0040] Furthermore, the mixed solution C is prepared by mixing hydrofluoric acid, nitric acid and pure water in a ratio of 3:6:11.

[0041] Furthermore, the mixed solution D is prepared by mixing hydrofluoric acid, nitric acid and glacial acetic acid in a ratio of 1:4:15.

[0042] Furthermore, the mixed solution E is prepared by mixing hydrofluoric acid, nitric acid and pure water in a ratio of 1:1:28.

[0043] Furthermore, in steps 7, 10, and 26, the ceramic surface of the ESC electrostatic adsorption plate is wiped multiple times, each time for 2-4 minutes and the dust-free cloth is replaced.

[0044] Furthermore, in step thirteen, it is ensured that the ceramic surface of the ESC electrostatic adsorption plate is immersed below the mixed solution D, and the other parts are kept above the liquid surface.

[0045] Furthermore, the ultrasonic cleaning in step 28 needs to be carried out in a clean room with a cleanliness level of at least 1000, with an ultrasonic frequency of 40000 Hz and an ultrasonic intensity of 8 + / - 2 w / inch. 2 ; Ultrasonic cleaning time: 28-32min; The cleaning water is ultrapure water with a conductivity of more than 18.1 megohms.

[0046] Furthermore, step 30 needs to be carried out in a clean room with a cleanliness level of at least Class 1000, and dried in a dust-free oven with high-purity nitrogen purged inside the dust-free oven, with the drying temperature set to 100-105° C. and the drying time set to 3-4 hours.

[0047] Compared with the prior art, the above technical solution adopted by the present invention has the following advantages: the process of the present invention removes the silicon, oxygen, titanium nitride and fluoride residual films deposited on the surface while fully protecting the component body from corrosion and loss, and effectively removes the color film on the surface caused by the high temperature of the machine. Finally, through the final ultrasonic cleaning in the clean room, the surface is absolutely clean and can meet the micro-environment use requirements in the equipment cavity.

[0048] Cleaning and refurbishing the ESC electrostatic adsorption plate of semiconductor plasma dry etching equipment can help semiconductor manufacturers greatly reduce production costs, save resources, and improve the utilization rate of product components. The price of each set of refurbished equipment components is only 1 / 80 to 1 / 100 of the purchase price of a new product, but the refurbished parts can achieve the same use effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 The figure shows a side view of the ESC electrostatic adsorption disk of the present invention;

[0050] Figure 2 The front view (with ceramic surface) of the ESC electrostatic adsorption disk of the present invention is shown;

[0051] Figure 3The figure shows the back view of the ESC electrostatic adsorption disk of the present invention;

[0052] Figure 4 Shown is a diagram of the helium hole flushing and purging fixture of the present invention. DETAILED DESCRIPTION

[0053] In order to make the purpose, technical solutions and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application, that is, the embodiments described are only part of the embodiments of the present application, not all of the embodiments.

[0054] Therefore, the following detailed description of the embodiments of the present application provided in the accompanying drawings is not intended to limit the scope of the present application for which protection is sought, but merely represents selected embodiments of the present application. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.

[0055] Example 1

[0056] This embodiment provides a process for removing silicon, oxygen, titanium nitride and fluoride deposited films deposited at high temperature on the surface of an electrostatic adsorption disk of an ESC of a semiconductor etching device, specifically comprising:

[0057] Step 1: Protect the electrode holes and helium holes on the back of the ESC electrostatic adsorption disk with acid- and alkali-resistant tape, and then protect the entire back and sides with acid- and alkali-resistant tape to prevent chemical liquids from corroding the body and electrode holes and helium holes during the cleaning process;

[0058] Step 2: Immerse the protected ESC electrostatic adsorption plate in 55°-65° pure water for 25-35 minutes, and bubble and stir the pure water at the same time, and use hot water to infiltrate the surface of the ESC electrostatic adsorption plate to improve the efficiency of subsequent chemical liquid film removal;

[0059] Step 3: Prepare a mixed solution A with a ratio of 2:3:5 of ammonia water, hydrogen peroxide and pure water;

[0060] Step 4: Take out the ESC electrostatic adsorption plate from the pure water, drain the residual liquid, and soak it in the mixed acid solution A for 3 to 4 hours to remove the fluoride and part of the titanium nitride residual film deposited on the surface of the ceramic plate of the ESC electrostatic adsorption plate;

[0061] Step 5: Take out the ESC electrostatic adsorption plate from the mixed solution A and rinse it with an air-water gun at a pressure of 0.4-0.5 MPa for 2-4 minutes.

[0062] Step 6: Prepare a mixed solution B with a ratio of 1:3:6 of ammonia water, hydrogen peroxide and pure water;

[0063] Step 7: After rinsing, use a dust-free cloth dipped in mixed solution B to wipe the ceramic surface of the ESC electrostatic adsorption disk. You can wipe it 4 times, changing the dust-free cloth every 2-4 minutes; further remove a small amount of fluoride and part of the titanium nitride residual film that may remain on the ceramic plate of the ESC electrostatic adsorption disk;

[0064] Step 8: After wiping, use an air-water gun to rinse the ceramic surface of the ESC electrostatic adsorption plate. The flushing pressure is 0.4-0.5 MPa and the flushing time is 2-4 minutes.

[0065] Step 9: Prepare a mixed solution C with a ratio of 3:6:11 of hydrofluoric acid, nitric acid and pure water;

[0066] Step 10: After rinsing, use a dust-free cloth dipped in mixed solution C to wipe the ceramic surface of the ESC electrostatic adsorption plate. You can wipe it 3 times, each time for 2-4 minutes and replace the dust-free cloth; mainly to remove titanium nitride and oxide residual film on the ceramic surface of the ESC electrostatic adsorption plate.

[0067] Step 11: After wiping, use an air-water gun to rinse the ceramic surface of the ESC electrostatic adsorption plate. The flushing pressure is 0.4-0.5 MPa and the flushing time is 2-4 minutes.

[0068] Step 12: Prepare a mixed solution D of hydrofluoric acid, nitric acid and glacial acetic acid in a ratio of 1:4:15;

[0069] Step 13: After rinsing, turn the ESC electrostatic adsorption plate upside down and immerse it in the mixed solution D. At this time, you only need to ensure that the front ceramic surface is immersed below the mixed solution D, and the other parts are kept above the liquid surface. The immersion time is 2-4 minutes; mainly remove silicon-containing compounds on the surface, such as polycrystalline silicon, single crystal silicon and some titanium nitride residual films;

[0070] Step 14: After soaking, use an air-water gun to rinse the ceramic surface of the ESC electrostatic adsorption plate. The flushing pressure is 0.4-0.5 MPa and the flushing time is 2-4 minutes.

[0071] Step 15: After rinsing, remove the acid- and alkali-resistant tape on the back and sides of the whole, and also remove the acid- and alkali-resistant tape on the helium hole;

[0072] Step 16: Use an air-water gun to rinse the entire ESC electrostatic adsorption plate with a flushing pressure of 0.4-0.5 MPa and a flushing time of 2-4 minutes;

[0073] Step 17: Install the helium hole flushing and purge fixture of the ESC electrostatic adsorption plate, and connect pure water to flush the helium hole. The flushing pressure is 0.1-0.2 MPa;

[0074] Step 18: Use a diamond grinding disc to grind the ceramic surface of the ESC electrostatic adsorption plate, and keep the helium holes flushed with pure water until the grinding is completed; the purpose of grinding is mainly to remove the color film and residual film caused by high temperature on the ceramic surface. Because the helium holes are distributed on the surface of the ceramic plate, pure water needs to be injected from the bottom during grinding to keep pure water flowing out of the front helium holes to prevent the debris caused by grinding from clogging the helium holes;

[0075] Step 19: After polishing, use an air-water gun to rinse the entire ESC electrostatic adsorption plate. The flushing pressure is 0.4-0.5 MPa and the flushing time is 2-4 minutes.

[0076] Step 20: Stop flushing the helium hole with pure water and remove the ESC electrostatic adsorption plate from the fixture;

[0077] Step 21: Use industrial scouring pad to polish the anodized surface of the side and back of the ESC electrostatic adsorption plate. This step uses No. 7447 industrial scouring pad for polishing, which is mainly used to remove the marks and dirt on the anodized surface of the side and the aluminum surface of the back of the ESC electrostatic adsorption plate when it is installed on the machine;

[0078] Step 22: After polishing, use an air-water gun to rinse the entire ESC electrostatic adsorption plate. The flushing pressure is 0.4-0.5 MPa and the flushing time is 2-4 minutes.

[0079] Step 23: After rinsing, use a high-purity nitrogen gun to dry the moisture on the surface of the ESC electrostatic adsorption plate and in the helium holes;

[0080] Step 24: Protect the back and sides of the ESC electrostatic adsorption plate with acid- and alkali-resistant tape to prevent chemical liquid from corroding the sides and back of the body during the cleaning process;

[0081] Step 25: prepare a mixed solution E of hydrofluoric acid, nitric acid and pure water in a ratio of 1:1:28;

[0082] Step 26: Use a dust-free cloth to dip in the mixed solution E to wipe the ceramic surface of the ESC electrostatic adsorption plate. You can wipe it twice, each time for 2-4 minutes and replace the dust-free cloth; it is used to remove the debris caused by grinding and the very small amount of residual film that may remain;

[0083] Step 27: After wiping, use an air-water gun to rinse the ceramic surface of the ESC electrostatic adsorption plate. The flushing pressure is 0.4-0.5 MPa and the flushing time is 2-4 minutes.

[0084] Step 28: After rinsing, remove the acid-alkali resistant tape on the back and sides of the ESC electrostatic adsorption plate;

[0085] Step 29: Use an air-water gun to rinse the entire ESC electrostatic adsorption plate, with a flushing pressure of 0.4-0.5 MPa and a flushing time of 2-4 minutes;

[0086] Step 30: Use ultrasonic waves to clean the ESC electrostatic adsorption plate. This step needs to be performed in a clean room with a cleanliness level of at least 1000; ultrasonic frequency: 40000Hz; ultrasonic intensity: 8+ / -2w / inch 2 ; Ultrasonic cleaning time: 30 minutes; The cleaning water is ultrapure water with a conductivity of 18.1 megohms or more; Ultrasonic cleaning is used to remove micron-sized dust particles on the surface of the ESC electrostatic adsorption disk to avoid uneven plasma etching caused by dust particles when the machine is on;

[0087] Step 31: After ultrasonic cleaning, remove the acid-alkali resistant tape from the electrode holes on the back of the ESC electrostatic adsorption disk;

[0088] Step 32: Final drying of the ESC electrostatic adsorption plate: This step needs to be carried out in a clean room with a cleanliness level of at least 1000, and is dried in a dust-free oven. The inside of the dust-free oven is purged with high-purity nitrogen (purity above 99.99%), and the drying temperature is set to 100-105°C, and the drying time is set to 3-4 hours. If the moisture is not fully dried, the water molecule particles on the machine will cause uneven plasma etching.

[0089] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. A process for removing high-temperature deposited silicon, oxygen, titanium nitride and fluoride films on the surface of an electrostatic adsorption disk of a semiconductor etching device ESC, characterized in that: include: Step 1: Protect the electrode holes and helium holes on the back of the ESC electrostatic adsorption disk with acid- and alkali-resistant tape, and then protect the entire back and sides with acid- and alkali-resistant tape; Step 2: Immerse the protected ESC electrostatic adsorption plate in 55°-65° pure water for a period of time, and bubble and stir the pure water during the immersion period; Step 3: preparing a mixed solution A; the mixed solution A is prepared by mixing ammonia water, hydrogen peroxide and pure water in a ratio of 2:3:5; Step 4: Take out the ESC electrostatic adsorption plate from the pure water, drain the remaining liquid, and soak it in mixed solution A for 3 to 4 hours; Step 5: Take out the ESC electrostatic adsorption plate from the mixed solution A and rinse it with an air-water gun at a pressure of 0.4-0.5 MPa; Step 6: preparing a mixed solution B; the mixed solution B is prepared by mixing ammonia water, hydrogen peroxide and pure water in a ratio of 1:3:6; Step 7: After rinsing, use a dust-free cloth to dip in mixed solution B and wipe the ceramic surface of the ESC electrostatic adsorption plate; Step 8: After wiping, use an air-water gun to rinse the ceramic surface of the ESC electrostatic adsorption plate at a pressure of 0.4-0.5 MPa; Step nine: preparing a mixed solution C; the mixed solution C is prepared by mixing hydrofluoric acid, nitric acid and pure water in a ratio of 3:6:11; Step 10: After rinsing, use a dust-free cloth to dip in mixed solution C and wipe the ceramic surface of the ESC electrostatic adsorption plate; Step 11: After wiping, use an air-water gun to rinse the ceramic surface of the ESC electrostatic adsorption plate at a pressure of 0.4-0.5 MPa; Step 12: preparing a mixed solution D; the mixed solution D is prepared by mixing hydrofluoric acid, nitric acid and glacial acetic acid in a ratio of 1:4:15; Step 13: After rinsing, place the ESC electrostatic adsorption plate upside down and soak it in the mixed solution D for a period of time; Step 14: After soaking, use an air-water gun to rinse the ceramic surface of the ESC electrostatic adsorption plate at a pressure of 0.4-0.5 MPa; Step 15: After rinsing, remove the acid- and alkali-resistant tape on the back and sides of the whole, and also remove the acid- and alkali-resistant tape on the helium hole; Step 16: Use an air-water gun to flush the entire ESC electrostatic adsorption plate at a pressure of 0.4-0.5 MPa; Step 17: Install the helium hole flushing and purge fixture of the ESC electrostatic adsorption plate, and connect pure water to flush the helium hole. The flushing pressure is 0.1-0.2 MPa; Step 18: Use a diamond grinding disc to grind the ceramic surface of the ESC electrostatic adsorption disk, and keep flushing the helium hole with pure water until the grinding is completed; Step 19: Use an air-water gun to flush the entire ESC electrostatic adsorption plate at a pressure of 0.4-0.5 MPa; Step 20: Stop flushing the helium hole with pure water and remove the ESC electrostatic adsorption plate from the fixture; Step 21: Use an industrial sponge to polish the anodized surface on the side and back of the ESC electrostatic adsorption plate; Step 22: After polishing, use an air-water gun to rinse the entire ESC electrostatic adsorption plate at a pressure of 0.4-0.5 MPa; Step 23: After rinsing, use a high-purity nitrogen gun to dry the moisture on the surface of the ESC electrostatic adsorption plate and in the helium holes; Step 24: Protect the back and sides of the ESC electrostatic adsorption plate with acid- and alkali-resistant tape; Step 25: preparing a mixed solution E; the mixed solution E is prepared by mixing hydrofluoric acid, nitric acid and pure water in a ratio of 1:1:28; Step 26: Use a dust-free cloth to dip in the mixed solution E and wipe the ceramic surface of the ESC electrostatic adsorption plate; Step 27: After wiping, use an air-water gun to rinse the ceramic surface of the ESC electrostatic adsorption plate at a pressure of 0.4-0.5 MPa; Step 28: After rinsing, remove the acid-alkali resistant tape on the back and sides of the ESC electrostatic adsorption plate; Step 29: Use an air-water gun to flush the entire ESC electrostatic adsorption plate at a flushing pressure of 0.4-0.5 MPa; Step 30: Use ultrasonic waves to clean the ESC electrostatic adsorption plate; Step 31: After ultrasonic cleaning, remove the acid-alkali resistant tape from the electrode holes on the back of the ESC electrostatic adsorption disk; Step 32: Dry the ESC electrostatic adsorption plate.

2. The process for removing high-temperature deposited silicon, oxygen, titanium nitride and fluoride films on the surface of the electrostatic adsorption disk of the semiconductor etching equipment ESC according to claim 1 is characterized in that: In steps 7, 10, and 26, wipe the ceramic surface of the ESC electrostatic adsorption plate multiple times, each time for 2-4 minutes and replace the dust-free cloth.

3. The process for removing high-temperature deposited silicon, oxygen, titanium nitride and fluoride films on the surface of the electrostatic adsorption disk of the semiconductor etching equipment ESC according to claim 1, characterized in that: In step 13, ensure that the ceramic surface of the ESC electrostatic adsorption plate is immersed below the mixed solution D, and the other parts are kept above the liquid surface.

4. The process for removing high-temperature deposited silicon, oxygen, titanium nitride and fluoride films on the surface of the electrostatic adsorption disk of semiconductor etching equipment ESC according to claim 1, characterized in that: The ultrasonic cleaning in step 28 needs to be carried out in a clean room with a cleanliness level of 1000 or above, with an ultrasonic frequency of 40000Hz and an ultrasonic intensity of 6-10w / inch. 2 ; Ultrasonic cleaning time: 28-32min; The cleaning water is ultrapure water with a conductivity of more than 18.1 megohms.

5. The process for removing high-temperature deposited silicon, oxygen, titanium nitride and fluoride films on the surface of the electrostatic adsorption disk of the semiconductor etching equipment ESC according to claim 1, characterized in that: Step 30 needs to be carried out in a clean room with a cleanliness level of 1000 or above, and is dried in a dust-free oven with high-purity nitrogen purged inside. The drying temperature is set to 100-105° C. and the drying time is set to 3-4 hours.