A core making method for enhanced cooling of 100-ton ductile iron container castings

By adopting a double casting system and the cooling method of 'cold iron + core bone internal ventilation cycle' in a 100-ton ductile iron core spent fuel container, the graphite distortion and low-temperature toughness reduction caused by long solidification time are solved, and the castings are efficient The cooling and mechanical properties are improved, ensuring the international advanced level of castings.

CN115870473BActive Publication Date: 2024-11-15ZHENGZHOU RES INST OF MECHANICAL ENG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211672453.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-26
Publication Date
2024-11-15
Estimated Expiration
2042-12-26

AI Technical Summary

Technical Problem

Due to the long solidification time of 100-ton ductile iron core spent fuel container castings are prone to graphite distortion, spherification decline, reduction in graphite sphere count, component segregation and uneven tissue, resulting in the reduction of low-temperature toughness.

Method used

Using a dual casting system and the 'cold iron + core bone internal ventilation circulation' cooling method, the cooling is enhanced through chromite sand filling and circulation ventilation pipes to ensure internal heat dissipation and exhaust of the castings, and the combination of graphite cold iron and cast iron cold iron is used to cool. Structure, control ventilation cycle time and temperature, and improve the cooling speed and mechanical properties of the castings.

Benefits of technology

It effectively improves the low-temperature and high toughness and mechanical properties of the castings, ensures the microstructure uniformity of the ductile iron container and the international advanced performance indicators, shortens the cooling time of the castings, and avoids graphite distortion and spheroidization decay.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115870473B_ABST
    Figure CN115870473B_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of 100-ton ductile iron nuclear spent fuel container castings, and particularly relates to a core making method for enhanced cooling of 100-ton ductile iron container castings. The molten iron is poured into a casting cavity through a double pouring system, the outer wall of the casting is cooled by a metal mold, the inner side of the casting is cooled by "chill iron + ventilation circulation inside the core bone", the top of the core bone is cooled by a graphite chill iron, the body is cooled by a cast iron chill iron, chromite ore sand is filled between the chill irons and between the chill iron and the core bone, air holes are provided around the core bone, a circulating ventilation pipeline is placed inside the core bone for enhanced cooling, the ventilation circulation inside the core bone can be stopped 5 to 6 hours after the pouring is completed (more than 1 hour after the temperature measuring point of the metal mold rises above 100°C), and the outer mold can be removed to take out the casting when the temperature of the temperature measuring point of the metal mold is less than 50°C. The invention safely and effectively solves the problems of spheroidization decay, graphite distortion, small number of graphite balls, severe component segregation, etc. caused by long solidification time of 100-ton ductile iron castings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of 100-ton ductile iron nuclear spent fuel container castings, and in particular relates to a core making method for enhancing cooling of 100-ton ductile iron container castings. Background Art

[0002] There are different types of large-scale nuclear spent fuel metal storage and transportation containers in the world, such as sandwich lead screen stainless steel, ductile iron, carbon steel multi-layer wrapping, metal ceramics, forged steel, etc. Ductile iron containers have high integrity and obvious economy, and have short manufacturing and processing cycles. They are currently an important technical route for metal transport containers in the world. The 100-ton ductile iron nuclear spent fuel container casting has a large tonnage (about 130 t) and thick wall thickness (about 500 mm). The thickness at the hot spot exceeds 650 mm. It is an ultra-large section ductile iron casting. In addition to having good room and high temperature strength and room temperature impact properties, it must also meet the use requirements of good low-temperature impact and fracture toughness under -40℃ conditions. The performance index requirements are: room temperature tensile properties, tensile strength ≥300 MPa, yield strength ≥200 MPa, elongation ≥12%; 100℃ tensile properties, tensile strength ≥280MPa, yield strength ≥180MPa, elongation; room temperature impact toughness ≥12J / cm2; -40℃ impact toughness ≥4J / cm2, -40℃ fracture toughness ≥50MPa√m.

[0003] The container casting is in the shape of a cylinder. The iron part has a large heat capacity, slow cooling speed, and long solidification time, which makes it easy for graphite distortion, spheroidization decline, reduction of graphite nodules, component segregation, coarse and uneven organization, and pearlite in the last solidification part to occur in the center of the wall thickness or hot node of the casting, resulting in a decrease in mechanical properties, especially low-temperature toughness. Using a metal mold on the outside of the casting cylinder is an effective measure to improve the heat dissipation of the casting outward, but because the heat inside the cylinder is concentrated in the core and the heat dissipation space is small, developing a safe and efficient enhanced cooling core making method is one of the key measures to ensure uniform organization and performance inside and outside the casting cylinder. Summary of the invention

[0004] The purpose of the present invention is to provide a core making method for enhanced cooling of 100-ton ductile iron container castings, enhance internal heat dissipation and exhaust, and safely and effectively solve the problems of spheroidization decay, graphite distortion, small number of graphite balls, severe component segregation, etc. of ultra-thick and large-section ductile iron due to long solidification time, thereby ensuring the microstructure and mechanical properties of low-temperature and high-toughness ductile iron. The manufactured ductile iron container is sampled from a 500mm section from the outside to the inside, and the microstructure and mechanical properties reach the advanced level of similar international castings.

[0005] To achieve the above object, the technical scheme adopted by the present invention is: a core making method for enhanced cooling of a 100-ton ductile iron container casting, wherein the molten iron is simultaneously poured into the casting cavity through a double pouring system, the outer wall of the casting is cooled by a metal mold, and the inner side of the casting is cooled by "chill iron + ventilation circulation inside the core bone", the top of the core bone is cooled by a graphite chill iron, the body is cooled by a cast iron chill iron, 30-50 mm thick chromite sand is filled between the chill irons, and 100 mm thick chromite sand is filled between the chill iron and the core bone, air holes are opened around the core bone, and a circulating ventilation pipe is placed inside the core bone for enhanced cooling, 5-6 hours after the pouring is completed (more than 1 hour after the metal mold temperature measuring point is heated to more than 100°C), the ventilation circulation inside the core bone is stopped, and when the temperature of the metal mold temperature measuring point is less than 50°C, the outer mold is removed to take out the casting;

[0006] The casting cavity includes a sand box at the bottom, pouring channels on both sides of the sand box, and a core located at the upper center of the sand box, which is composed of a core bone, chill and chromite sand, and an inner wall of a cylindrical metal mold located outside the core. A cavity is formed between the inner wall of the metal mold and the core. An air vent is also provided on the metal mold at the top of the outer wall of the metal mold. A graphite chill is provided on the top of the outer side of the core bone, and a cast iron chill is provided around the core bone. A cavity is provided in the sand box at the bottom of the core bone. The sand box is filled with resin sand except for the pouring channel and the cavity, and a ventilation circulation component is provided inside the core bone.

[0007] Furthermore, the ventilation circulation component includes an air inlet pipe and an air outlet pipe, the bottom of the air inlet pipe extends out of the bottom of the core bone and is connected to the outside world, the top of the air inlet pipe extends upward to the graphite cold iron at the top of the core bone, the upper part of the air outlet pipe is located at the lower middle part of the core bone, the bottom outlet of the air outlet pipe extends out of the core bone and is connected to the outside world, and the parts of the air inlet pipe and the air outlet pipe located inside the core bone are provided with through holes around them.

[0008] Furthermore, through holes are also provided on the side walls of the core bone, and temperature measuring points are also provided on the outer wall of the cylindrical metal mold at the hot node position. The temperature measuring points are arranged at the hot nodes of the metal mold corresponding to the casting to control the start and stop of the ventilation cycle.

[0009] Furthermore, the cast iron chill is gray cast iron with a thickness of 0.5~0.6T (T is the main wall thickness of the casting). The cast iron chill needs to be derusted and dried before use. There are 12 pieces of chill in the circumferential direction of the container body, which are divided into 13 layers in the axial direction. The chill is filled with chromite sand at an axial interval of 30mm and a circumferential interval of 30mm; the graphite chill C% is ≥98, and the volume density is g / mm 3≥1.65, the working surface requires machining, and its surface must be flat and smooth without holes, inclusions, cracks, etc.; the non-working surface retains cutting marks to increase the surface roughness, and the roughness is >Ra150; it is strictly forbidden to use liquids during machining or grinding. Graphite chills enhance heat transfer on the one hand, and improve the yield of castings on the other hand, and facilitate the removal of castings in post-processing procedures; the core bone is carbon steel with a wall thickness of 20~30mm, and the chill and the outer wall of the core bone are filled with 100mm molding sand to improve the yield of the chill structure of the casting shrinkage.

[0010] Furthermore, the core bone is a round tube with a ring tray on the top, the tray is evenly distributed with holes of φ30mm, the air inlet and outlet of the air inlet pipe are 200~300mm away from the top tray, and the air inlet of the air outlet pipe is 3500~4000mm away from the top tray.

[0011] The present invention has the advantages that:

[0012] 1. The present invention adopts the developed low-temperature and high-toughness 100-ton ductile iron nuclear spent fuel container casting enhanced cooling method, uses high-purity pig iron and other high-quality raw materials to prepare high-temperature pure raw iron liquid, and uses 0.055%~0.065% Mg residual content for spheroidization inoculation treatment, "outer wall metal mold + inner wall cold iron + core bone internal circulation ventilation" combined enhanced cooling process molding, monitors the temperature of the outer wall of the metal mold, quantitatively controls the ventilation termination time and the metal mold boxing time, samples and analyzes the casting body, and takes three groups of samples from the top and body of the casting for detection (such as Figure 4 ), the matrix structure is all ferrite, and the mechanical properties of the main body sample are: room temperature tensile strength ≥351MPa, yield strength ≥229MPa, elongation ≥19%; 100℃ tensile strength ≥330MPa, yield strength ≥193MPa, elongation after fracture ≥22.5%; room temperature impact ≥25J / cm 2 , -40℃ low temperature impact ≥7.1J / cm 2 ; -40℃ fracture toughness ≥72.19MPa√m;

[0013] 2. The present invention develops an enhanced cooling core-making method for a hundred-ton ductile iron container of "core bone internal circulation ventilation + top graphite + cast iron body chiller": the core bone supports the chiller to improve the core strength; chromite sand is filled between the chillers to ensure that the core has good yieldability and good cooling capacity; holes are opened around the core bone and the top tray, and the gas generated during the pouring process is introduced into the core bone, effectively preventing the gas generated by the core from invading the casting; two high and low ventilation circulation pipes are used inside the core bone, which, on the one hand, take away the heat inside the core bone, form a temperature gradient between the chiller and the inner cavity of the core bone, strengthen the heat dissipation of the chiller inward, and at the same time discharge the gas inside the core bone. The developed enhanced cooling core-making method is safe and efficient, improves the cooling rate of the casting, and obtains a hundred-ton low-temperature and high-toughness ductile iron container casting with excellent organizational properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 The figure is a schematic diagram of the shape and structure of a 100-ton ductile iron nuclear spent fuel container casting prepared by the present invention.

[0015] Figure 2 It is a schematic diagram of the casting cavity modeling of the enhanced cooling casting process in the present invention.

[0016] Figure 3 It is a schematic diagram of the structure of the core bone internal circulation ventilation component.

[0017] Figure 4 It is a schematic diagram of the sampling location for casting testing. DETAILED DESCRIPTION

[0018] As shown in the figure, a core making method for enhanced cooling of a 100-ton ductile iron container casting is provided. The molten iron is simultaneously poured into the casting cavity 1 through a double pouring system 8. The outer wall of the casting is cooled by a metal mold 2. The inner side of the casting is cooled by "chill iron + ventilation circulation inside the core bone". A graphite chill iron 4 is used on the top of the core bone 11, and a cast iron chill iron 5 is used on the body. A 30-50 mm thick chromite sand is filled between the chill irons, and a 100 mm thick chromite sand is filled between the chill iron and the core bone. Air holes 11-1 are provided around the core bone, and a circulating ventilation pipe is placed inside the core bone for enhanced cooling. After 5-6 hours of pouring (more than 1 hour after the metal mold temperature measuring point 3 is heated to more than 100°C), the ventilation circulation inside the core bone is stopped, and when the temperature at the temperature measuring point is less than 50°C, the outer mold is removed to take out the casting.

[0019] The casting cavity 1 includes a sand box 6 located at the bottom, a pouring channel located on both sides of the sand box 6, and also includes a core composed of a core bone 11 and chills 4 and 5, an inner wall of a cylindrical metal mold located outside the core, a cavity is formed between the inner wall of the metal mold and the core, and an air outlet 12 is also provided on the top of the metal mold, a graphite chill is provided on the top of the outer side of the core bone, a cast iron chill is provided around the core bone, and a cavity is provided in the sand box at the bottom of the core bone, and the positions of the sand box except the pouring channel and the cavity are all filled with resin sand 7, and a ventilation circulation component is provided inside the core bone; the ventilation circulation component includes an air inlet pipe 10 and an air outlet pipe 9, the bottom 10-1 of the air inlet pipe extends out of the bottom of the core bone and is connected to the outside, the top 10-2 of the air inlet pipe extends upward to the graphite chill at the top of the core bone, the upper part 9-1 of the air outlet pipe is located in the middle and lower part of the core bone, and the outlet of the bottom 9-2 of the air outlet pipe extends out of the core bone and is connected to the outside. The outside world is connected, and the air inlet and outlet pipes are provided with through holes around the parts located in the core bone; the side walls of the core bone are also provided with through holes 11-1, and the outer wall of the cylindrical metal mold is also provided with a temperature measuring point 3 at the hot node position. The temperature measuring point is arranged at the hot node of the metal mold corresponding to the casting to control the start and stop of the ventilation cycle. The core bone is a circular tube with an annular tray on the top, and the tray is evenly distributed with holes of φ30mm. The air inlet and outlet of the air inlet pipe are 200~300mm away from the top tray, and the air inlet of the air outlet pipe is 3500~4000mm away from the top tray; the cast iron chiller is HT200 chiller with a thickness of 0.5~0.6T. The cast iron chiller needs to be derusted and dried before use. There are 12 pieces of chillers circumferentially on the container body, which are divided into 13 layers in the axial direction. The chillers are spaced 30mm in the axial direction and 30mm in the circumferential direction, and are filled with chromite sand; the graphite chiller C% ≥ 98, and the volume density is g / mm 3 ≥1.65, the working surface requires machining, and its surface must be flat and smooth without holes, inclusions, cracks, etc.; the non-working surface retains cutting marks to increase the surface roughness, and the roughness is >Ra150; it is strictly forbidden to use liquids during machining or grinding. Graphite chills enhance heat transfer on the one hand, and improve the yield of castings on the other hand, and facilitate the removal of castings in post-processing procedures; the core bone is carbon steel with a wall thickness of 20~30mm, and the chill and the outer wall of the core bone are filled with 100mm molding sand to improve the yield of the chill structure of the casting shrinkage.

[0020] When used specifically, the casting barrel enhanced cooling core making method is suitable for: Figure 2The molding process shown is that the outer wall of the casting is cooled by a metal mold, and the inner side of the casting adopts "chill iron + core bone internal ventilation circulation". The top graphite chill is used for the enhanced cooling core of the casting, and the body is made of cast iron chill. The chill is supported by the core bone. 30~50mm thick chromite sand needs to be filled between the chills, and 100mm thick chromite sand is filled between the chill and the core bone to increase the yield of the core. Air holes are opened around the core bone, and a circulating ventilation duct is placed inside the core bone. On the one hand, it strengthens cooling, and on the other hand, it discharges the gas generated by the heating of the core sand. Temperature measuring points are arranged at the hot nodes of the metal mold corresponding to the casting to control the start and stop of the ventilation cycle; the cast iron chill is made of gray cast iron material, and the thickness of the chill is 0.5~0.6T. The cast iron chill needs to be derusted and dried before use. There are 12 circumferential chills on the body of the container, which are divided into 13 layers in the axial direction. The chills are spaced 30mm in the axial direction and 30mm in the circumferential direction, and are filled with chromite sand molding. The graphite chilled iron C%≥98, volume density g / mm 3 ≥1.65. The working surface requires machining, and its surface must be smooth and free of holes, inclusions, cracks, etc.; the non-working surface retains cutting marks to increase the surface roughness, and the roughness is > Ra150; it is strictly forbidden to use liquids during machining or grinding. Graphite chilled iron enhances heat transfer on the one hand, and improves the yield of castings on the other hand, and facilitates the removal of castings in post-processing procedures; the core bone is carbon steel with a manufacturing wall thickness of 20~30mm. The chilled iron and the outer wall of the core bone are filled with 100mm molding sand to improve the shrinkage of the casting and the yield of the chilled iron structure; the ventilation circulation process inside the core bone is as follows Figure 3 As shown; the internal circulation ventilation pipeline of the core bone is made of ordinary carbon structural steel, one end of which is pre-buried in the center of the casting cavity and the other end passes through the bottom of the sand box, as shown in FIG. Figure 3 9 is the air outlet pipe, 10 is the air inlet pipe, the air inlet temperature is ≥100℃, and the ventilation device is turned on before pouring. The graphite chill is fixedly supported by the chill tray on the top of the core bone, and the tray is evenly distributed with φ30mm holes to enhance air permeability. The air outlet of the air inlet pipe is 200~300mm away from the top tray; the air inlet of the air outlet pipe is 3500~4000mm away from the top tray; the core bone is surrounded by air holes with a hole diameter of φ20~φ30mm, and the hole position radially corresponds to the center of the chill. The temperature measurement point is located on the outer wall of the metal mold at the hot node, such as Figure 2 As shown in 3. Before pouring, open the temperature measuring point 3 to measure the temperature, and the temperature fluctuation during the temperature measurement process is no more than 2°C. After 5 to 6 hours after pouring is completed (1 hour after the temperature at the temperature measuring point 3 exceeds 100°C during the heating process), the ventilation device can stop circulating ventilation. After pouring is completed, when the temperature at the temperature measuring point 3 exceeds the peak value and the temperature drops to below 50°C, remove the outer mold and take out the casting.

Claims

1. A core making method for enhanced cooling of 100-ton ductile iron container castings, characterized in that: The molten iron is poured into the casting cavity at the same time through a double pouring system. The outer wall of the casting is cooled by a metal mold, and the inner side of the casting is cooled by "chilled iron + ventilation circulation inside the core bone". The top of the core bone is made of graphite chilled iron, and the body is made of cast iron chilled iron. The space between the chilled irons is filled with 30-50mm thick chromite sand, and the space between the chilled iron and the core bone is filled with 100mm thick chromite sand. Air holes are opened around the core bone, and a circulating ventilation pipe is placed inside the core bone for enhanced cooling. After 5-6 hours of pouring, the temperature measuring point of the metal mold rises above 100℃ for more than 1 hour, and the ventilation circulation inside the core bone is stopped. When the temperature of the temperature measuring point of the metal mold is less than 50℃, the outer mold is removed to take out the casting. The casting cavity includes a sand box at the bottom, pouring channels on both sides of the sand box, and a core located at the upper center of the sand box, which is composed of a core bone, chill and chromite sand, and an inner wall of a cylindrical metal mold located outside the core, and a cavity is formed between the inner wall of the metal mold and the core. An air vent is also provided on the metal mold at the top of the outer wall of the metal mold, a graphite chill is provided on the top of the outer side of the core bone, a cast iron chill is provided around the core bone, and a cavity is provided in the sand box at the bottom of the core bone. The sand box is filled with resin sand except for the pouring channel and the cavity, and a ventilation circulation component is provided inside the core bone.

2. The core making method for enhanced cooling of 100-ton ductile iron container castings according to claim 1, characterized in that: The ventilation circulation component includes an air inlet pipe and an air outlet pipe. The bottom of the air inlet pipe extends out of the bottom of the core bone and is connected to the outside world. The top of the air inlet pipe extends upward to the graphite cold iron at the top of the core bone. The upper part of the air outlet pipe is located at the lower middle part of the core bone. The bottom outlet of the air outlet pipe extends out of the core bone and is connected to the outside world. Through holes are provided around the parts of the air inlet pipe and the air outlet pipe located inside the core bone.

3. The core making method for enhanced cooling of 100-ton ductile iron container castings according to claim 1, characterized in that: The side walls of the core are also provided with through holes, and the outer wall of the cylindrical metal mold is also provided with a temperature measuring point at the hot node position.

4. The core making method for enhanced cooling of 100-ton ductile iron container castings according to claim 1, characterized in that: The cast iron chill is grey cast iron with a thickness of 0.5-0.6T, where T is the main wall thickness of the casting. The graphite chill has a C% of ≥98 and a bulk density of g / mm 3 ≥1.65, the core is carbon steel, and the wall thickness is 20~30mm.

5. The core making method for enhanced cooling of 100-ton ductile iron container castings according to claim 1, characterized in that: The core bone is a round tube with a ring tray on the top, the tray is evenly distributed with φ30mm holes, the air inlet and outlet of the air inlet pipe are 200-300mm away from the top tray, and the air inlet of the air outlet pipe is 3500-4000mm away from the top tray.